A method for preparing TaC coating using ultrafine TaC powder
By preparing ultrafine TaC powder through chemical vapor deposition and forming a TaC coating through sintering, the problems of insufficient purity and density of TaC coatings in existing technologies are solved, enabling efficient and simple industrial production and improving the performance of TaC coatings.
Patent Information
- Application Number
- CN202411203939.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The purity and density of TaC coatings in existing technologies are not high, which affects their ability to improve the performance of carbon-based materials. The preparation methods are also complex and not suitable for industrial applications.
Ultrafine TaC powder was prepared by chemical vapor deposition and then used as raw material to form a TaC coating by sintering. The process included refining, feeding, preheating, first and second stage deposition, and recycling processes to control powder particle size and purity and avoid agglomeration.
High-purity TaC powder with uniform particle size was prepared, forming a more dense TaC coating, which improved the performance and functionality of carbon-based materials. The process is simple and suitable for industrial production.
Smart Images

Figure CN118702492B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of TaC powder preparation, in particular to a method for preparing a TaC coating with ultrafine TaC powder. Background Art
[0002] As the semiconductor field continues to increase its requirements for the use of carbon material devices, silicon carbide can no longer meet the requirements in some special scenarios. For example, at 1600°C, H2 will promote the gasification of silicon carbide, which will cause the silicon carbide coating to be slowly corroded, resulting in excessive differences in the surface roughness of the coating and uneven surface temperature distribution; or the silicon carbide coating will be corroded through, further quickly corroding the internal graphite substrate, leaving only a thin layer of silicon carbide coating on the surface.
[0003] TaC is one of the best candidate materials to replace silicon carbide. TaC is an ultra-high temperature material that can still be used normally above 2000°C. Depositing TaC on the surface of carbon-based materials to form a TaC coating can make the carbon material have good thermal shock resistance, oxidation resistance and excellent thermochemical stability. Therefore, TaC coatings are widely used in single crystal growth, epitaxy and other fields, which can reduce the impurity content of products, extend the service life of parts and components, and improve production efficiency. However, the current method for preparing TaC coatings is relatively simple, the process is difficult, and it is not very mature in industrial production. It cannot adapt well to the demand for TaC coatings in the prior art field. More importantly, the TaC purity and density of the TaC coatings prepared by the prior art are not high, which seriously affects the performance improvement of the TaC coating on carbon-based materials and reduces its functionality.
[0004] Therefore, a new method for preparing TaC coating is urgently needed to obtain TaC coating with higher purity and density. Summary of the invention
[0005] In order to improve the above problems existing in the prior art, the present invention provides a method for preparing ultrafine TaC powder and TaC coating thereof. The present invention uses TaC powder as raw material and adopts a sintering method to form a TaC coating, which has a simple process path and has the advantages of sustainable production and high production efficiency; and the TaC powder prepared by the method of the present invention has a more uniform and fine particle size, which can make the TaC coating formed by the TaC powder have higher purity and higher density, and the TaC powder formed by the chemical vapor deposition process is not easy to agglomerate, thereby improving the performance improvement of the TaC coating on carbon-based materials and its functionality.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a TaC coating from ultrafine TaC powder, the method comprising: forming TaC powder by chemical vapor deposition process; forming a TaC coating by sintering the TaC powder as a raw material; wherein the chemical vapor deposition process comprises the following steps:
[0007] A refinement process is performed to refine the tantalum source powder under a first protective gas; and a feeding process is performed to introduce the tantalum source powder at a first molar ratio under a carrier gas and a reducing gas; and a preheating process is performed to maintain a first time period at a first temperature; and a first-stage deposition process is performed to continue to introduce a carbon source gas at a second molar ratio under a second protective gas and maintain the second temperature for a second time period; and a second-stage deposition process is performed to decrease the temperature from the second temperature to a third temperature within a third time period; and a recovery process is performed to collect the TaC powder using a vacuum recovery device and neutralize the tail gas to obtain the TaC powder.
[0008] Through the above technical solution, the present invention has at least the following advantages compared with the prior art:
[0009] The TaC powder prepared by the chemical vapor deposition method can effectively improve the powder agglomeration problem. n H m -H2-Ar(X=F, Cl, Br, C n H m The TaC powder formed by chemical vapor deposition process in a system including one or more of CH4, C2H4, C2H6, C3H6 and C3H8 has a finer agglomerate particle size and its chemical formula is TaC x , where 0.9≤ x ≤1, there is no impurity phase such as Ta2C and C, and it has very high purity, thereby improving the performance improvement of TaC coating on carbon-based materials and its functionality; and the present invention uses TaC powder as a raw material to form the TaC coating by a sintering method, the process path is simple, and it has the advantages of sustainable production and high production efficiency, and has a wider application prospect.
[0010] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1This is one of the SEM images of TaC powder provided in one embodiment of the present invention.
[0012] Figure 2 The second SEM image of TaC powder provided in one embodiment of the present invention and its EDS element distribution map.
[0013] Figure 3 This is a first particle size distribution diagram of TaC powder provided in one embodiment of the present invention.
[0014] Figure 4 This is a second particle size distribution diagram of TaC powder provided in one embodiment of the present invention.
[0015] Figure 5 This is a diagram of the process equipment for preparing TaC powder provided by the present invention.
[0016] Figure 6 This is an optical microscope image of the appearance of a TaC coating provided in one embodiment of the present invention.
[0017] Figure 7 This is the SEM image of purchased micron-sized TaC powder. DETAILED DESCRIPTION
[0018] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0019] Compared with the direct preparation of TaC coatings based on chemical vapor deposition, the preparation of TaC coatings by sintering is less difficult in terms of process difficulty. In addition, the preparation of TaC coatings by chemical vapor deposition is not yet mature in industrial production. Therefore, the preparation of TaC coatings by sintering is a possible idea for coating preparation. The sintering method for preparing TaC coatings for semiconductor equipment first requires high-purity TaC powder with uniform powder particle size. However, the TaC powder commonly used at present is synthesized by vacuum heat treatment of Ta2O5 and C, which has a low purity and a certain amount of carbon and oxygen impurities due to incomplete reaction. The high synthesis temperature causes the powder to sinter and coarsen. If further purification is required, the steps are more complicated and the cost is significantly increased, which cannot better meet the needs of the existing technical field for TaC powder.
[0020] Therefore, based on the above problems, the present invention aims to prepare TaC powder with higher purity, ultrafine particle size and uniform particle size, so as to have better sintering performance and obtain a TaC coating with higher purity and better performance.
[0021] A first aspect of the present invention provides a method for preparing a TaC coating from ultrafine TaC powder, the method comprising: forming TaC powder by a chemical vapor deposition process; forming a TaC coating by a sintering method using the TaC powder as a raw material; wherein the chemical vapor deposition process comprises the following steps:
[0022] performing a refinement process to refine the tantalum source powder under a first protective gas; and,
[0023] performing a feeding process to introduce the tantalum source powder at a first molar ratio under a carrier gas and a reducing gas; and,
[0024] performing a preheating process, maintaining a first temperature for a first period of time; and,
[0025] performing a first stage deposition process, continuing to introduce the carbon source gas at a second molar ratio under a second protective gas, and maintaining the second temperature for a second period of time; and,
[0026] performing a second stage deposition process, decreasing the temperature from the second temperature to a third temperature within a third time period; and,
[0027] A recovery process is performed, the TaC powder is collected by using a vacuum recovery device, and the tail gas is neutralized to obtain the TaC powder.
[0028] The present invention adopts chemical vapor deposition method to prepare TaC powder, which can effectively improve the powder agglomeration problem. n H m -H2-Ar(X=F, Cl, Br, C n H m The TaC powder formed by chemical vapor deposition process in a system including one or more of CH4, C2H4, C2H6, C3H6 and C3H8 has a finer agglomerate particle size and its chemical formula is TaC x , where 0.9≤ x ≤1, no impurity phases such as Ta2C and C exist, and the purity is very high, thereby improving the performance improvement and functionality of the TaC coating on carbon-based materials; and the present invention uses homemade TaC powder as a raw material to form the TaC coating by a sintering method, the process path is simple, and it has the advantages of sustainable production and high production efficiency, and has a wider application prospect;
[0029] More importantly, compared with the direct preparation of TaC coating based on chemical vapor deposition, the method of first preparing TaC powder and then preparing TaC coating by sintering is less difficult in process and more mature in industrial production. Moreover, the TaC powder prepared by the chemical vapor deposition method provided by the present invention has higher purity and more uniform and fine powder. When combined with the use of sintering to prepare TaC coating, a TaC coating with higher purity and density can be formed, thereby further improving the functionality of the TaC coating.
[0030] Furthermore, according to the chemical vapor deposition process of the present invention, a refinement process is performed under the first protective gas to refine the tantalum source powder, so that the particle size of the reaction raw material can be controlled within an appropriate range. On the one hand, it can avoid the tantalum source powder from agglomerating due to its excessive size, and on the other hand, the tantalum source powder can be further refined to make the powder particle size distribution more uniform, and the reactivity of the tantalum source powder can be improved, so that the powder reacts more fully and thoroughly, thereby improving the purity of the TaC powder; further, in the process of performing the feeding process and the first stage deposition process, adjusting the first molar ratio and the second molar ratio related to the tantalum source powder and the carbon source gas can further improve the reactivity of the tantalum source powder and the carbon source gas, so that the particle size distribution of the TaC powder is more uniform and the particle size is finer during the nucleation and crystallization growth process, and by adjusting the above-mentioned molar ratio, a TaC powder with higher purity can be obtained.
[0031] According to the method of the present invention, the chemical formula of the TaC powder is TaC x , where 0.9≤ x ≤1; the agglomerate particle size of the TaC powder is ≤1μm; the distribution kurtosis of the first particle size distribution peak is 0.85-0.96, and the distribution kurtosis of the second particle size distribution peak is 0.9-1.02; the distribution width of the first particle size distribution peak is 0.075-0.112, and the distribution width of the second particle size distribution peak is 0.083-0.092. Specifically, Figure 3 and Figure 4 As shown, the TaC powder prepared by the present invention can contain two different particle size distribution peaks, that is, bimodal distribution, and the powder can contain two particle groups with different particle sizes. The agglomerate particle size of the TaC powder prepared by the present invention is less than or equal to 1 μm, indicating that the particle size is small and fine, and by making the TaC powder contain two different particle size distribution peaks, the overall packing density of the powder can be effectively improved, which is conducive to the densification of the powder during the sintering process, and the particle size distribution ranges of the two peaks are narrow, and the particle size distribution is relatively uniform, which further improves the density of the TaC coating.
[0032] According to the method of the present invention, the TaC powder includes a first agglomerate particle and a second agglomerate particle, the size of the first agglomerate particle is submicron, and the size of the second agglomerate particle is nanometer. The two different distribution peaks of the TaC powder prepared by the method of the present invention can correspond to agglomerate particles of two size levels, that is, coarse powder and fine powder are included at the same time, the first agglomerate particle is coarse powder, the size is at the submicron level, and the second agglomerate particle is fine powder, the size is at the nanometer level, and the two agglomerate particles can fill the gaps between each other, and the gaps left between the large particle agglomerates can be filled by the small particle agglomerates, so that the density of the TaC coating after sintering can be improved, and the close stacking of large and small particles not only reduces the internal gaps, but also enhances the contact area between the agglomerate particles, thereby improving the internal bonding force of the coating, and then can also avoid the incorporation of impurity phases, further improve the purity of the TaC coating, and can also make the final TaC coating have more excellent anti-corrosion and anti-oxidation properties, and improve the performance improvement of the TaC coating on carbon-based materials and its functionality.
[0033] In a specific embodiment, the size of the first agglomerated particles is 100nm-1000nm, and exemplarily, the size of the first agglomerated particles is 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, and the size of the second agglomerated particles is 1nm-100nm, and exemplarily, the size of the second agglomerated particles is 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 99nm, 100nm. The present invention can further improve the compactness of the TaC coating after sintering by adjusting the size range of the first agglomerated particles and the second agglomerated particles, and is more in line with the process path of the sintering method, does not need to increase the sintering temperature, and has the advantages of sustainable production and high production efficiency. In addition, it should be noted that although the sizes of the first agglomerated particles and the second agglomerated particles both include the endpoint 100nm, in a specific embodiment, they do not overlap.
[0034] In a specific embodiment, based on the mass content of the TaC powder, the mass content of the first agglomerate particles is 70wt%-90wt%, and for example, the mass content of the first agglomerate particles can be 70wt%, 75wt%, 80wt%, 85wt%, and 90wt%; the mass content of the second agglomerate particles is 10wt%-30wt%, and for example, the mass content of the second agglomerate particles can be 10wt%, 15wt%, 20wt%, 25wt%, and 30wt%. By accurately controlling the proportion of agglomerate particles of different particle sizes, the performance of the TaC coating can be further optimized, and the uniformity of different positions of the TaC coating can be ensured.
[0035] In a specific embodiment, during the thinning process, the first protective gas includes Ar, and the first protective gas is high-purity Ar, 5N or more, to ensure that no impurities or doping are introduced.
[0036] In a specific embodiment, during the refinement process, the tantalum source powder includes one or more of TaCl5, TaBr5 and TaF5. In a preferred embodiment, the tantalum source powder is TaCl5. Since TaCl5 is very easy to hydrolyze in the air and produce HCl gas (TaBr5 and TaF5 also have the same problem), it needs to be processed in a container filled with protective gas, and the powder is ball milled (including but not limited to roller ball milling, planetary ball milling, vibration ball milling, discharge plasma ball milling) to further refine the powder, making the powder particle size distribution more uniform and improving the reactivity of the powder.
[0037] In a specific embodiment, the particle size of the tantalum source powder obtained after the refinement process is ≤500μm. Exemplarily, the particle size of the tantalum source powder can be 500μm, 450μm, 400μm, 350μm, 300μm, 250μm, 200μm, 180μm, 150μm, 100μm, 75μm, 50μm. In a preferred embodiment, the particle size of the tantalum source powder is 75μm-200μm. In the early stage of generating TaC powder, refining the particle size of the reaction material tantalum source powder can make the subsequent reaction proceed more smoothly and generate TaC powder of suitable particle size.
[0038] In a specific embodiment, during the feeding process, the carrier gas includes Ar.
[0039] In one embodiment, during the feeding process, the reducing gas includes hydrogen.
[0040] In a specific embodiment, the first molar ratio is the ratio of the molar contents of the tantalum source powder, the reducing gas and the carrier gas, and the first molar ratio is 1:(1-2):(0.5-2). Exemplarily, the first molar ratio can be 1:1:0.5, 1:1:2, 1:2:0.5, 1:2:2. The ratio of the molar contents of tantalum source powder, reducing gas and carrier gas can reflect the feeding speed of tantalum source powder. The faster the feeding speed of tantalum source powder is, the more powder passes through the same area in the pipeline, so a higher temperature is required to completely sublimate the powder in the middle of the pipeline. Otherwise, it is easy to cause the obtained TaC powder to have uneven particle size or be too large, which affects the particle size uniformity and fineness of TaC powder. Therefore, the present invention further controls the first molar ratio so that the feeding speed of tantalum source powder is within a suitable range, which can further improve the uniformity of TaC powder and improve the particle size of TaC powder, making it smaller and finer, and more in line with the preparation conditions of sintering method, thereby generating a TaC coating with better purity and density.
[0041] In a specific embodiment, during the preheating process, the first temperature is 400°C-500°C; illustratively, the first temperature can be 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C. In a specific embodiment, the first time period is 5s-10s. It should be noted that the first temperature is the heating temperature set by the process equipment. During the preheating process, the tantalum source powder fed in will undergo a morphological transformation at the first temperature set by the process equipment. For example, TaCl5(s) will first sublimate into TaCl5(g) and then into TaCl4(g) during the preheating process. By setting the heating temperature of the equipment at the first temperature, it can be ensured that the internal temperature of the tantalum source powder during the morphological transformation is maintained within the range of 150°C-300°C, so as to ensure sufficient morphological transformation, thereby obtaining higher gas reaction activity, providing a reaction basis for the subsequent rapid reaction with the carbon source gas, and further optimizing various aspects of the performance of the TaC powder.
[0042] In a specific embodiment, the second protective gas Ar and the carbon source gas include one or more of CH4, C2H4, C2H6, C3H6 and C3H8.
[0043] In a specific embodiment, the second molar ratio is the ratio of the molar content of the second protective gas to the total molar content of the tantalum source powder, the carbon source gas, the reducing gas and the carrier gas, and the second molar ratio is 1:(2-5). When the molar ratio is greater than 1:2, the feeding speed inside the pipeline will be too fast, and too much powder will pass through the same area in the pipeline, which may easily lead to uneven powder particle size. When the molar ratio is less than 1:5, the feeding speed inside the pipeline will be too slow, which will extend the process path time and also cause the reactivity of the powder to decrease, resulting in uneven powder particle size. Therefore, by controlling the second molar ratio within an appropriate range, the uniformity of the TaC powder can be further improved.
[0044] In a specific embodiment, during the execution of the first stage deposition process, the second temperature is 1000°C-2000°C, and the second time period is 10s-15s; during the execution of the second stage deposition process, the third temperature is 500°C-1500°C, and the third time period is 10s-15s; the second temperature is greater than the third temperature.
[0045] It should be noted that the second temperature and the third temperature are consistent with the first temperature, and are both heating temperatures set by the process equipment, and the second temperature in the method of the present invention is greater than the third temperature. Specifically, the source gas, tantalum source powder and carbon source gas that are about to react will first complete the initial reaction in the first temperature area (including the complete sublimation of the tantalum source powder and the reduction of the tantalum source, etc.), and convert all the raw materials into gas, which is conducive to the uniformity of the reaction; a rapid reaction occurs in the high temperature area maintained at the second temperature, including the gradual reduction of the tantalum source and the decomposition of CH4, the synthesis of TaC, and crystallization and growth as the reaction proceeds, and then the generated TaC powder is quickly sent to the low temperature area set to the third temperature for rapid cooling. The higher the third temperature, the longer the time the powder stays in the high temperature area, and the coarseness of the powder can be controlled. The lower the temperature, the finer the generated powder. The large flow of Ar allows the TaC powder to cool rapidly, which can ensure the formation of TaC powder, rather than directly forming a TaC coating.
[0046] According to the method of the present invention, a process apparatus diagram for preparing TaC powder by chemical vapor deposition process is shown in FIG. Figure 5 As shown, the reaction vessel used in the process of preparing TaC powder by chemical vapor deposition process of the present invention also includes but is not limited to vacuum sintering furnace, hot pressing sintering furnace, hot isostatic pressing sintering furnace and spark plasma sintering furnace commonly used in the art.
[0047] According to the method of the present invention, the sintering method includes one or more of gas pressure sintering, hot pressing sintering, hot isostatic pressing sintering, spark plasma sintering and microwave sintering.
[0048] According to the method of the present invention, the sintering method comprises the following steps:
[0049] The TaC powder and the silane coupling agent are uniformly mixed in a mass ratio of (20-80):1 to prepare a mixed powder, and polyvinyl butyral and dioctyl phthalate are uniformly mixed in a mass ratio of (2-8):1 to prepare an adhesive;
[0050] 10wt%-15wt% of the adhesive and 90wt%-85wt% of the mixed powder are uniformly mixed to form a slurry, and the slurry is coated on the pretreated substrate;
[0051] The substrate coated with the slurry is placed in a sintering furnace for sintering to obtain the TaC coating.
[0052] According to the method of the present invention, the silane coupling agent includes KH-550, and the main function of the silane coupling agent is to modify the surface of the TaC powder so that the TaC powder can be stably and evenly dispersed, reduce the agglomeration of ultrafine powder, and improve the uniformity and consistency of the TaC coating.
[0053] In a specific embodiment, the ratio of TaC powder to silane coupling agent can be 20:1, 30:1, 40:1, 50:1, 60:1, 70:1, or 80:1.
[0054] In a specific embodiment, the skim ratio of polyvinyl butyral to dioctyl phthalate can be 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, or 8:1.
[0055] In a specific embodiment, 10wt%-15wt% of the adhesive and 90wt%-85wt% of the mixed powder are uniformly mixed to form a slurry, which is then coated on a pretreated substrate. The formulation of the slurry is critical to the performance of the final coating, and different binders and dispersants will affect the adhesion, hardness and corrosion resistance of the coating. The slurry is coated on the pretreated substrate, which can be done by dipping, spraying, brushing, printing or spin coating, depending on the shape and size of the substrate and the required coating thickness.
[0056] According to the method of the present invention, during the sintering process, the sintering temperature is controlled at 1800°C-2400°C. For example, the sintering temperature may be 1800°C, 1900°C, 2000°C, 2100°C, 2200°C, 2300°C, 2400°C, and the sintering time is controlled at 0.2h-4h.
[0057] According to the method of the present invention, in the process of forming the TaC coating by the sintering method using the TaC powder as a raw material, the TaC powder is melted and then recrystallized to form TaC grains, and the TaC coating contains the TaC grains, and the size of the TaC grains is 5μm-30μm. Specifically, in the process of forming the TaC coating by the sintering method using the TaC powder as a raw material, the binder will be removed, and the TaC powder will undergo mutual bonding between particles at the specific sintering temperature set above, forming grains with a size of 5μm-30μm (such as Figure 6 As shown in the figure, the grains are coarse and fine, the size of the coarse grains is 15μm-30μm, and the size of the fine grains is 5μm-15μm, thereby achieving further densification of the TaC coating.
[0058] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0059] Unless otherwise specified, the materials and instruments used in the following examples are commercially available.
[0060] Example 1
[0061] 1. For preparing TaC powder, specifically comprising the following steps:
[0062] 1. Raw material powder tantalum source powder required for preparing TaC powder (the particle size of the final tantalum source powder is required to be 500μm or less and the purity is above 99.9%):
[0063] The sealed TaCl5 powder and the ball mill are placed in a glove box filled with Ar for loading and unloading operations. After the ball mill is closed and tightened, the ball mill is placed in a ball mill to ball mill the powder;
[0064] 2. The raw material after ball milling is introduced into the deposition chamber of the chemical vapor deposition process by screw feeding, and the first protective gas Ar and the reducing gas H2 are introduced, and the first molar ratio of TaCl5:H2:Ar=1:1:1 is ensured, and then the gas and powder in the deposition chamber are preheated so that the first temperature is controlled within the range of 420±4°C and maintained for 10s;
[0065] 3. Then, a high-concentration carbon source gas CH4 and a second protective gas Ar are provided into the deposition chamber, and the second molar ratio of the gas flow rate is ensured to be 1:5. Then, the reaction source gas is reacted in the high-temperature zone (the second temperature is set to 1200°C) for 15 seconds, and then the generated material is transferred to the low-temperature zone (the third temperature is set to 800°C) within 10 seconds for rapid cooling through the fluidity of the gas. Finally, the HCl gas and powder are sucked in through the collecting device, and the vacuum pump will suck the HCl gas and TaC powder to the rear end, and the powder is recovered by the powder recovery device to obtain TaC powder; wherein, the agglomerate particle size of the TaC powder prepared in Example 1 is less than 1 μm. After screening by a sieve, the submicron agglomerated particles account for about 80wt%, and the nano-scale agglomerated particles account for about 20wt%, wherein the SEM image of the nano-scale agglomerated particles is as follows: Figure 1 As shown; SEM image of TaC powder prepared in Example 1 and its EDS element distribution map, as shown Figure 2 As shown, it can be seen that the generated TaC powder has a finer agglomerate particle size, as well as very high purity and uniformity;
[0066] In addition, it should be noted that the TaC powder used for the preparation of the TaC coating has a bimodal distribution. After being screened by a sieve, the particle size distribution diagrams of the TaC powders measured are as follows: Figure 3 , Figure 4 As shown, the distribution kurtosis of the first particle size distribution peak of the TaC powder is 0.90, the distribution width of the first particle size distribution peak is 0.092, the distribution kurtosis of the second particle size distribution peak is 0.95, and the distribution width of the second particle size distribution peak is 0.089.
[0067] 2. Preparation steps of TaC coating:
[0068] 1. The TaC powder synthesized in the above step 1 is mixed with the silane coupling agent KH-550 at a mass ratio of 50:1 to make a mixed powder, and polyvinyl butyral and dioctyl phthalate are mixed at a mass ratio of 5:1 to make an adhesive, and a ball mill is used to ensure that the powder is fully dispersed and there is no agglomeration;
[0069] 2. 15wt% of the above-mentioned adhesive and 85wt% of the above-mentioned mixed powder were mixed evenly to form a slurry, and the slurry was coated on the pretreated substrate by spin coating. The coated substrate was then treated at 170°C for 2h and then placed in a sintering furnace for sintering and densification. The sintering temperature was set to 2000°C. After sintering for 2h, a TaC coating was obtained, and its optical microscope microscopic picture was observed, as shown in FIG. Figure 6As shown, it can be found that the TaC grains in the formed TaC coating are closely connected and have excellent compactness. In addition, the grains are coarse and fine, with coarse grains of about 15-30 μm and fine grains of about 5-15 μm. The average size of the formed TaC grains is 15 μm.
[0070] Example 2 Group
[0071] The second embodiment group was carried out with reference to the first embodiment, except that the setting temperature of the second temperature in the first stage deposition process was changed, specifically:
[0072] Embodiment 2a, changing the setting temperature of the second temperature in the first stage deposition process to 1000° C.;
[0073] Embodiment 2b, changing the setting temperature of the second temperature in the second stage deposition process to 1500° C.;
[0074] In Example 2c, the setting temperature of the second temperature in the second stage deposition process is changed to 2000°C.
[0075] Example 3 Group
[0076] The third embodiment group is carried out with reference to the first embodiment, except that the setting temperature of the second temperature in the first stage deposition process and / or the setting temperature of the third temperature in the second stage deposition process are changed at the same time, specifically:
[0077] Embodiment 3a, changing the setting temperature of the third temperature in the second stage deposition process to 500° C.;
[0078] In Example 3b, the setting temperature of the second temperature in the first stage deposition process is changed to 1800° C., and the setting temperature of the third temperature in the second stage deposition process is changed to 1500° C.
[0079] Example 4 Group
[0080] Example 4 was carried out with reference to Example 1, except that the control range of the first temperature was changed during the preheating process, specifically:
[0081] Embodiment 4a, the first temperature in the preheating process is controlled within the range of 480±4°C;
[0082] Embodiment 4b, the first temperature in the preheating process is controlled within the range of 250±4°C;
[0083] In Example 4c, the first temperature in the preheating process is controlled within the range of 550±4°C.
[0084] Example 5 Group
[0085] Example 5 was carried out with reference to Example 1, except that during the feeding process, the first molar ratio of the tantalum source powder was changed, specifically:
[0086] Example 5a, in the process of changing the feeding process, the first molar ratio of the tantalum source powder is TaCl5:H2:Ar=1:2:2;
[0087] Example 5b, in the process of changing the feeding process, the first molar ratio of the tantalum source powder TaCl5:H2:Ar=1:0.5:0.5.
[0088] Example 6 Group
[0089] Example 6 was carried out in accordance with Example 1, except that the second molar ratio of the carbon source gas introduced during the first stage deposition process was changed, specifically:
[0090] Example 6a, in the process of changing the feeding process, the second molar ratio of the introduced carbon source gas is 1:2;
[0091] In Example 6b, during the process of changing the feeding process, the second molar ratio of the introduced carbon source gas is 1:1.
[0092] Example 7 Group
[0093] Example 7 was carried out with reference to Example 1, except that the sintering temperature during the preparation of the TaC coating was changed, specifically:
[0094] Example 7a, changing the sintering temperature during the preparation of the TaC coating to 1800°C;
[0095] Example 7b, the sintering temperature in the preparation process of the TaC coating is changed to 2300°C.
[0096] Comparative Example 1
[0097] Comparative Example 1 was carried out in accordance with Example 1, except that commercially available TaC powder was used. The SEM image of the powder is shown in FIG. Figure 7 As shown, the average particle size of the raw material used for preparing the TaC coating is 1.5±0.8μm.
[0098] Comparative Example 2
[0099] Comparative Example 2 was carried out with reference to Example 1, except that commercially available TaC powder was used. The SEM image of the powder is shown in FIG. Figure 7 As shown, the average particle size of the raw material for preparing the TaC coating is 1.5±0.8 μm, and the sintering temperature during the preparation of the TaC coating is changed to 2300°C.
[0100] Comparative Example 3
[0101] Comparative Example 3 was carried out with reference to Example 1, except that the setting temperature of the third temperature in the second stage deposition process was changed to 1200°C.
[0102] Test Case
[0103] The specific particle size or grain size of the TaC powder and TaC coating prepared in the above embodiments and comparative examples is recorded in Table 1; the TaC coating prepared in the above embodiments and comparative examples is subjected to purity test, open porosity test and bonding strength test respectively, wherein the purity test adopts glow discharge mass spectrometry (GDMS) to detect the purity of the corresponding coating; the open porosity adopts the vacuum method: the sample is dried in an oven at 100°C and weighed to a constant weight, and the dried sample is weighed on a precision electronic balance, that is, the weight of the sample in the air m1 (dry weight); the sample is placed in a container and placed in a vacuum device, vacuumed to -0.1MPa, and maintained for 15 minutes. Then, distilled water is slowly injected until the sample is completely submerged, and then taken out after being maintained for 10 minutes, and the above sample is gently placed in the hanging basket of the electronic balance, and the floating amount of the sample is weighed while immersed in water m2; the sample is taken out of the water and the excess droplets on the surface are carefully wiped with a wet towel, and the liquid in the pores cannot be sucked out, and the saturated weight in the air m3 is immediately weighed. Open porosity = (m3-m1) / (m3-m2)×100%; The bonding strength test refers to the fine ceramic interface tensile and shear bond strength test method-cross method (GB / T 31541-2015) to test the bonding strength between the substrate and the TaC coating; all the above test results are also recorded in Table 1.
[0104] Table 1
[0105]
[0106] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing TaC coating from ultrafine TaC powder, characterized in that: The method comprises: forming TaC powder by chemical vapor deposition process; using the TaC powder as raw material and forming TaC coating by sintering method; wherein, The chemical vapor deposition process comprises the following steps: performing a refinement process to refine the tantalum source powder under a first protective gas; and, performing a feeding process to introduce the tantalum source powder at a first molar ratio under a carrier gas and a reducing gas; and, performing a preheating process, maintaining a first temperature for a first period of time; and, performing a first stage deposition process, continuing to introduce the carbon source gas at a second molar ratio under a second protective gas, and maintaining the second temperature for a second period of time; and, performing a second stage deposition process, decreasing the temperature from the second temperature to a third temperature within a third time period; and, Performing a recovery process, using a vacuum recovery device to collect the TaC powder, and neutralizing the tail gas, so as to obtain the TaC powder; During the thinning process, the first protective gas includes Ar, and the tantalum source powder includes one or more of TaCl5, TaBr5 and TaF5; The particle size of the tantalum source powder obtained after the refinement process is ≤500 μm; During the feeding process, the carrier gas includes Ar, and the reducing gas includes H2; The first molar ratio is the ratio of the molar contents of the tantalum source powder, the reducing gas, and the carrier gas, and the first molar ratio is 1:(1-2):(0.5-2); During the preheating process, the first temperature is 400° C.-500° C., and the first time period is 5s-10s; During the first stage of the deposition process, the second temperature is 1000°C-2000°C, and the second time period is 10s-15s; during the second stage of the deposition process, the third temperature is 500°C-1500°C, and the third time period is 10s-15s; the second temperature is greater than the third temperature; During the first stage deposition process, the second protective gas includes Ar, and the carbon source gas includes one or more of CH4, C2H4, C2H6, C3H6 and C3H8; The second molar ratio is the ratio of the molar content of the second protective gas to the total molar content of the tantalum source powder, the carbon source gas, the reducing gas and the carrier gas, and the second molar ratio is 1:(2-5); The agglomerate particle size of the TaC powder is ≤1 μm.
2. The method for preparing TaC coating from ultrafine TaC powder according to claim 1, characterized in that: The chemical formula of the TaC powder is TaC x , where 0.9≤x≤1; The TaC powder has a first particle size distribution peak and a second particle size distribution peak, the distribution kurtosis of the first particle size distribution peak is 0.85-0.96, and the distribution kurtosis of the second particle size distribution peak is 0.9-1.02; the distribution width of the first particle size distribution peak is 0.075-0.112, and the distribution width of the second particle size distribution peak is 0.083-0.
092.
3. The method for preparing a TaC coating from ultrafine TaC powder according to claim 1 or 2, characterized in that: The TaC powder comprises first agglomerate particles and second agglomerate particles, the first agglomerate particles are submicron-sized, and the second agglomerate particles are nano-sized; And / or, the size of the first agglomerated particles is 100nm-1000nm, and the size of the second agglomerated particles is 1nm-100nm; And / or, based on the mass content of the TaC powder, the mass content of the first agglomerate particles accounts for 70wt%-90wt%, and the mass content of the second agglomerate particles accounts for 10wt%-30wt%.
4. The method for preparing TaC coating from ultrafine TaC powder according to claim 1, characterized in that: The sintering method includes one or more of gas pressure sintering, hot pressing sintering, hot isostatic pressing sintering, spark plasma sintering and microwave sintering.
5. The method for preparing TaC coating from ultrafine TaC powder according to claim 1, characterized in that: The sintering method comprises the following steps: The TaC powder and the silane coupling agent are uniformly mixed in a ratio of (20-80):1 to prepare a mixed powder, and polyvinyl butyral and dioctyl phthalate are uniformly mixed in a ratio of (2-8):1 to prepare an adhesive; 10wt%-15wt% of the adhesive and 90wt%-85wt% of the mixed powder are uniformly mixed to form a slurry, and the slurry is coated on the pretreated substrate; The substrate coated with the slurry is placed in a sintering furnace for sintering to obtain the TaC coating.
6. The method for preparing TaC coating from ultrafine TaC powder according to claim 5, characterized in that: During the sintering process, the sintering temperature is controlled at 1800° C.-2400° C., and the sintering time is controlled at 0.2 h-4 h; And / or, in the process of forming the TaC coating by the sintering method using the TaC powder as a raw material, the TaC powder is melted and then recrystallized to form TaC grains, the TaC coating contains the TaC grains, and the size of the TaC grains is 5μm-30μm.