A kind of polyimide graphene gel powder and its preparation method and application

By preparing polyimide/graphene gel powder, the problem of insufficient electromagnetic interference shielding performance of polyurethane materials is solved, and the mechanical properties and electromagnetic shielding performance of the material are improved, which are suitable for 3D printing and electromagnetic wave shielding.

CN118702962BActive Publication Date: 2024-11-29SUZHOU GANGRUITONG NANO MATERIALS TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411208464.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-29
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Existing polyurethane materials have poor electromagnetic interference shielding performance, making it difficult to take into account both electromagnetic interference shielding and mechanical properties.

Method used

Using the preparation method of polyimide/graphene gel powder, the graphene hydrogel is first prepared and impregnated with polyamic acid salt to form a gel material with high stability and porous structure, which improves its mechanical properties and Electromagnetic shielding performance.

Benefits of technology

It significantly improves the mechanical properties and electromagnetic shielding performance of the material, meets the high-precision requirements of 3D printing and the electromagnetic wave reflection loss ability, and enhances the shielding effect of electromagnetic waves.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118702962B_ABST
    Figure CN118702962B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of honeycomb materials, and particularly relates to a polyimide / graphene gel powder, a preparation method and an application thereof. The present invention uses polyethylene glycol and graphene oxide as raw materials to first prepare a graphene hydrogel. Polyethylene glycol, as a good modifier, is not only conducive to the dispersion of graphene, but also can improve the stability of the graphene hydrogel structure. Polyamic acid salt is added dropwise to the graphene hydrogel solution so that the polyamic acid salt fully infiltrates the inside of the graphene hydrogel to construct an internal network of the gel. The graphene hydrogel impregnation polyamic acid salt process not only further improves the mechanical properties of the gel material, but also improves the compatibility of graphene with polyurethane thermoplastic materials, which is conducive to meeting the process of 3D printing secondary processing. In addition, the post-impregnation graphene hydrogel can further reduce the pore size and increase the number of pore walls, thereby improving its reflection loss capability and improving the electromagnetic shielding performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of honeycomb materials, and in particular to a polyimide / graphene gel powder and a preparation method and application thereof. Background Art

[0002] 3D printing, also known as additive manufacturing technology, is an advanced manufacturing technology that uses three-dimensional software model files as the basis to manufacture complex physical parts by printing materials layer by layer and stacking them. After decades of rapid development, 3D printing technology has been well applied in scientific research, manufacturing, architecture, art, medicine, aerospace, film and television, etc. 3D printing technology does not require traditional tools and complex processing technology, which can greatly shorten the production cycle of products and reduce production costs. At present, the available materials for 3D printing mainly include polymers, metals, ceramics, composite materials, etc. Among them, 3D printing polymer materials are the earliest and most widely used 3D printing materials, accounting for more than 70% of the current 3D printing material market.

[0003] Thermoplastic polyurethane elastomer (thermoplastic polyurethane) refers to a class of elastomeric block polymers containing repeated carbamate functional groups on the main chain of the macromolecule. Its raw materials are usually oligomer polyols, polyisocyanates, chain extenders / cross-linkers and a small amount of additives. Compared with other raw materials that can be used for 3D printing (such as polylactic acid, polycarbonate, nylon, etc.), the biggest advantage of thermoplastic polyurethane materials is that their soft and hard segments are composed of different materials, which makes them have both the high elasticity of rubber and the high strength of plastic. By controlling the composition and proportion of the soft segment and the hard segment, various thermoplastic polyurethane products with diverse structures and wide applications can be synthesized. In addition, the wear resistance, oil resistance, weather resistance, tensile strength, hardness range and other properties of 3D printing thermoplastic polyurethane materials are all at an excellent level compared with similar products. In summary, thermoplastic polyurethane is an elastomeric material with excellent comprehensive performance. It is one of the selected raw materials for 3D printing technology and has a wide range of applications in the fields of machinery and electronic equipment. However, due to the inherent properties of plastic products, the electromagnetic shielding performance of electronic products prepared therefrom is poor. Electromagnetic pollution can cause strong electromagnetic interference between electronic devices, leading to electromagnetic information leakage and threatening the human body. Therefore, it is urgent to develop new and efficient electromagnetic protection materials to improve their shielding and protection effects against electromagnetic waves.

[0004] Electromagnetic interference can be effectively controlled by using electromagnetic shielding materials. Electromagnetic shielding materials are generally divided into metal type shielding materials, intrinsic conductive polymer type shielding materials, conductive polymer type composite shielding materials and multifunctional electromagnetic shielding materials. According to the different types of filling materials, they can also be divided into metal fillers, carbon nanofillers and conductive polymer materials. With the continuous advancement of electromagnetic protection technology, the demand for shielding materials is also increasing. Therefore, the future development direction is to compound materials with different properties to prepare composite materials with multiple functions. Summary of the invention

[0005] In view of this, the present invention provides a polyimide / graphene gel powder and a preparation method and application thereof, which aims to solve the technical problem that the existing polyurethane shielding materials cannot take into account both electromagnetic interference shielding performance and mechanical performance.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a method for preparing a polyimide / graphene gel powder, comprising the following steps:

[0008] (1) dispersing graphene oxide, a reducing agent and polyethylene glycol in deionized water to obtain a graphene oxide mixed solution, sealing the mixed solution and placing the mixed solution in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:(0.01-0.1);

[0009] (2) dispersing a diamine monomer and a dianhydride monomer as raw materials in an organic solvent for polycondensation to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder;

[0010] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:(0.1-1);

[0011] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0012] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0013] Graphene aerogel has the characteristics of low density, high porosity, good resilience and adsorption. Graphene with a three-dimensional structure is constructed by integrating two-dimensional graphene. The three-dimensional porous structure and the excellent properties of graphene itself are combined to give it the structural characteristics of low density and large specific surface area, overcome the defect of easy stacking of two-dimensional graphene, and make it have better mechanical and conductive properties. At the same time, this porous structure can increase the reflection of electromagnetic waves in the hole, so that it has a wider application in the field of electromagnetic shielding. However, the compatibility of pure graphene aerogel with polymers such as polyurethane is poor, and it is difficult to meet the high-precision requirements of products in the 3D printing process. The main chain of polyimide molecules is mainly composed of rigid five-membered heterocyclic rings and aromatic rings, which makes the PI molecular chain very rigid. In addition, the high conjugation effect of aromatic heterocyclic rings enhances the interaction between molecular chains, thereby giving PI high mechanical properties and high / low temperature resistance. The composite preparation of polyimide and graphene to prepare aerogel not only solves the problem of graphene compatibility, but also improves the mechanical properties of gel powder through the formation of polymer network.

[0014] There are many preparation technologies for polyimide / graphene gel materials in the prior art. However, they generally adopt in-situ gel formation method (CN106750290A, CN110357067A, etc.), graphene aerogel impregnation method (CN112094426A), polyamide acid hydrogel loaded graphene method (CN116218018A). The above-mentioned process either prepares polyamide acid gel or graphene aerogel first, or prepares aerogel after blending polyamide acid with graphene, and the matrix structure is a polymer, the structure is unstable, and the mechanical properties are poor. When used for 3D printing melt reprocessing, structural damage will occur. In order to overcome this problem, the present invention uses polyethylene glycol and graphene oxide as raw materials to first prepare graphene hydrogel and construct a graphene-based gel material. The graphene prepared by the redox method has more active groups on its surface. Polyethylene glycol, as a good modifier, is not only conducive to the dispersion of graphene, but also can form hydrogen bonds with oxygen-containing functional groups such as carboxyl or hydroxyl groups on the surface of graphene, thereby enhancing the interaction between graphene sheets and improving the stability of the graphene hydrogel structure. The number average molecular weight of polyethylene glycol can be 400-5000, specifically PEG400, PEG600, PEG800, PEG1000, PEG2000, PEG5000, etc.

[0015] The polyamic acid salt aqueous solution is added dropwise to the graphene hydrogel solution, so that the polyamic acid salt fully infiltrates the inside of the graphene hydrogel and constructs the internal network of the gel. Compared with the addition of graphene to polyamic acid hydrogel, the impregnation of polyamic acid in graphene aerogel, and the in-situ preparation of hydrogel process, the graphene hydrogel impregnation polyamic acid salt process not only further improves the mechanical properties of the gel material, but also improves the compatibility of graphene with thermoplastic materials such as polyurethane, which is conducive to meeting the process of secondary processing of 3D printing. In addition, post-impregnation of graphene hydrogel can further reduce the pore size and increase the number of pore walls, thereby improving its reflection loss ability and improving electromagnetic shielding performance. The use of tertiary amines and polyamic acid to react to prepare polyamic acid salts is conducive to improving the solubility of polyamic acid substances, reducing the viscosity of the solution, and improving the wettability of polyamic acid and graphene hydrogel.

[0016] In one embodiment, the graphene oxide concentration in the graphene oxide mixed solution in step (1) is 0.5-2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:(0.1-0.5).

[0017] In one embodiment, the heating reaction temperature in step (1) is 60-90° C. and the time is 1-4 h.

[0018] In one embodiment, the dianhydride monomer in step (2) is at least one of 4,4'-biphenyl ether dianhydride, biphenyl tetracarboxylic dianhydride, 1,2,4,5-pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, bisphenol A type diether dianhydride, 4,4-oxydiphthalic anhydride, and 1,2,4,5-cyclohexane tetracarboxylic dianhydride; the diamine monomer is at least one of p-phenylenediamine, m-phenylenediamine, diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ether, and 4,4'-diaminodiphenylmethane. The molar ratio of the dianhydride monomer to the diamine monomer is (0.95-1.05): (0.95-1.05).

[0019] In one embodiment, the organic solvent in step (2) is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and N-methylpyrrolidone.

[0020] In one embodiment, the tertiary amine in step (3) is at least one of triethylamine, tripropylamine and triethanolamine.

[0021] In one embodiment, in step (3), the mass ratio of the polyamic acid powder to the tertiary amine is 1:(0.3-0.6).

[0022] In a second aspect, the present invention provides a polyimide / graphene gel powder, which is prepared by the above-mentioned method for preparing the polyimide / graphene gel powder.

[0023] In a third aspect, the present invention provides an application of polyimide / graphene gel powder, and uses the polyimide / graphene gel powder in the field of 3D printing polyurethane materials.

[0024] In a fourth aspect, the present invention provides a 3D printing polyurethane material, comprising the following components in parts by weight:

[0025] 100 parts of thermoplastic polyurethane elastomer; 5-10 parts of polyimide / graphene gel powder; 1-5 parts of flow modifier.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The preparation process is simple and easy to operate, which is a convenient and efficient preparation method;

[0028] (2) First, graphene hydrogel is prepared to construct a graphene-based gel material. Polyethylene glycol, as a good modifier, is not only conducive to the dispersion of graphene, but also can form hydrogen bonds with oxygen-containing functional groups such as carboxyl or hydroxyl groups on the surface of graphene, thereby enhancing the interaction between graphene sheets and improving the stability of the graphene hydrogel structure.

[0029] (3) The graphene hydrogel impregnation process with polyamic acid salt not only further improves the mechanical properties of the gel material, but also improves the compatibility of graphene with thermoplastic materials such as polyurethane, which is conducive to meeting the process of secondary processing of 3D printing.

[0030] (4) Impregnating the prepared anisotropic graphene hydrogel with polyamic acid salt can further reduce the pore size and increase the number of pore walls, thereby improving its reflection loss capability and electromagnetic shielding performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope image of the polyimide / graphene gel powder prepared in Example 5;

[0032] Figure 2 This is a scanning electron microscope image of the polyimide / graphene gel powder prepared in Comparative Example 1;

[0033] Figure 3 This is a graph of the X-band electromagnetic shielding performance of the 3D printed polyurethane material prepared in Examples 1-4;

[0034] Figure 4 This is a graph of the X-band electromagnetic shielding performance of 3D printed polyurethane materials prepared in Examples 5-7 and Comparative Examples 1-3. DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0036] Example 1

[0037] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0038] (1) Graphene oxide, a reducing agent and polyethylene glycol PEG800 are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and placed in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol PEG800 is 1:0.02; the concentration of graphene oxide in the graphene oxide mixed solution is 0.7 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.1; the heating reaction temperature is 60°C and the time is 4 hours;

[0039] (2) using diamine monomer and dianhydride monomer as raw materials and dispersing them in N,N-dimethylformamide for polycondensation to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.03; the dianhydride monomer is 4,4'-biphenyl ether dianhydride; and the diamine monomer is 4,4'-diaminodiphenyl ether;

[0040] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine triethylamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.3; the mass ratio of graphene oxide to polyamic acid powder is 1:0.3;

[0041] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0042] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0043] A 3D printing polyurethane material comprises the following components in parts by weight:

[0044] 100 parts of thermoplastic polyurethane elastomer; 5 parts of polyimide / graphene gel powder; 1 part of zinc stearate.

[0045] Example 2

[0046] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0047] (1) Graphene oxide, a reducing agent and polyethylene glycol PEG800 are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and placed in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol PEG800 is 1:0.1; the graphene oxide concentration in the graphene oxide mixed solution is 1.8 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.5; the heating reaction temperature is 90°C and the time is 1 h;

[0048] (2) using diamine monomer and dianhydride monomer as raw materials and dispersing them in N-methylpyrrolidone for polycondensation reaction to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.03; the dianhydride monomer is 3,3',4,4'-benzophenonetetracarboxylic dianhydride; and the diamine monomer is a mixture of m-phenylenediamine and diaminodiphenyl sulfone in a molar ratio of 1:1;

[0049] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine tripropylamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.6; the mass ratio of graphene oxide to polyamic acid powder is 1:0.6;

[0050] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0051] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0052] A 3D printing polyurethane material comprises the following components in parts by weight:

[0053] 100 parts of thermoplastic polyurethane elastomer; 8 parts of polyimide / graphene gel powder; 2 parts of zinc stearate.

[0054] Example 3

[0055] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0056] (1) Graphene oxide, a reducing agent and polyethylene glycol PEG800 are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and placed in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol PEG800 is 1:0.03; the concentration of graphene oxide in the graphene oxide mixed solution is 1.1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.2; the heating reaction temperature is 70°C and the time is 3 h;

[0057] (2) using diamine monomer and dianhydride monomer as raw materials and dispersing them in N,N-dimethylacetamide to carry out polycondensation reaction to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.01; the dianhydride monomer is 1,2,4,5-cyclohexanetetracarboxylic dianhydride; and the diamine monomer is p-phenylenediamine;

[0058] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine triethanolamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.4; the mass ratio of graphene oxide to polyamic acid powder is 1:0.4;

[0059] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0060] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0061] A 3D printing polyurethane material comprises the following components in parts by weight:

[0062] 100 parts of thermoplastic polyurethane elastomer; 6 parts of polyimide / graphene gel powder; 3 parts of zinc stearate.

[0063] Example 4

[0064] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0065] (1) Graphene oxide, a reducing agent and polyethylene glycol PEG800 are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and placed in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol PEG800 is 1:0.08; the concentration of graphene oxide in the graphene oxide mixed solution is 1.5 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.4; the heating reaction temperature is 80°C and the time is 2 h;

[0066] (2) using diamine monomer and dianhydride monomer as raw materials and dispersing them in N,N-dimethylformamide to carry out polycondensation reaction to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.03; the dianhydride monomer is bisphenol A type diether dianhydride, and the diamine monomer is diaminodiphenyl sulfone;

[0067] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine triethylamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.5; the mass ratio of graphene oxide to polyamic acid powder is 1:0.5;

[0068] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0069] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0070] A 3D printing polyurethane material comprises the following components in parts by weight:

[0071] 100 parts of thermoplastic polyurethane elastomer; 8 parts of polyimide / graphene gel powder; 4 parts of zinc stearate.

[0072] Example 5

[0073] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0074] (1) Graphene oxide, a reducing agent and polyethylene glycol PEG800 are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and placed in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol PEG800 is 1:0.05; the concentration of graphene oxide in the graphene oxide mixed solution is 1.2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 h;

[0075] (2) dispersing a diamine monomer and a dianhydride monomer as raw materials in N,N-dimethylformamide to carry out a polycondensation reaction to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.01; the dianhydride monomer is 4,4'-biphenyl ether dianhydride, and the diamine monomer is 4,4'-diaminodiphenylmethane;

[0076] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine triethylamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.4; the mass ratio of graphene oxide to polyamic acid powder is 1:0.5;

[0077] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0078] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0079] A 3D printing polyurethane material comprises the following components in parts by weight:

[0080] 100 parts of thermoplastic polyurethane elastomer; 7 parts of polyimide / graphene gel powder; 3 parts of zinc stearate.

[0081] Example 6

[0082] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0083] (1) Graphene oxide, a reducing agent and polyethylene glycol PEG800 are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and placed in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol PEG800 is 1:0.05; the concentration of graphene oxide in the graphene oxide mixed solution is 1.2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 h;

[0084] (2) dispersing a diamine monomer and a dianhydride monomer as raw materials in N,N-dimethylformamide to carry out a polycondensation reaction to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.01; the dianhydride monomer is 4,4'-biphenyl ether dianhydride, and the diamine monomer is 4,4'-diaminodiphenylmethane;

[0085] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine triethylamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.4; the mass ratio of graphene oxide to polyamic acid powder is 1:0.1;

[0086] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0087] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0088] A 3D printing polyurethane material comprises the following components in parts by weight:

[0089] 100 parts of thermoplastic polyurethane elastomer; 7 parts of polyimide / graphene gel powder; 3 parts of zinc stearate.

[0090] Example 7

[0091] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0092] (1) Graphene oxide, a reducing agent and polyethylene glycol PEG800 are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and placed in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol PEG800 is 1:0.05; the concentration of graphene oxide in the graphene oxide mixed solution is 1.2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 h;

[0093] (2) dispersing a diamine monomer and a dianhydride monomer as raw materials in N,N-dimethylformamide to carry out a polycondensation reaction to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.01; the dianhydride monomer is 4,4'-biphenyl ether dianhydride, and the diamine monomer is 4,4'-diaminodiphenylmethane;

[0094] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine triethylamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.4; the mass ratio of graphene oxide to polyamic acid powder is 1:1;

[0095] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0096] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0097] A 3D printing polyurethane material comprises the following components in parts by weight:

[0098] 100 parts of thermoplastic polyurethane elastomer; 7 parts of polyimide / graphene gel powder; 3 parts of zinc stearate.

[0099] Comparative Example 1

[0100] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0101] (1) Graphene oxide and a reducing agent are dispersed in deionized water to obtain a graphene oxide mixed solution, which is sealed and placed in an oven for heating to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide mixed solution is 1.2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 h;

[0102] (2) dispersing a diamine monomer and a dianhydride monomer as raw materials in N,N-dimethylformamide to carry out a polycondensation reaction to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.01; the dianhydride monomer is 4,4'-biphenyl ether dianhydride, and the diamine monomer is 4,4'-diaminodiphenylmethane;

[0103] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine triethylamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.4; the mass ratio of graphene oxide to polyamic acid powder is 1:0.5;

[0104] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0105] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0106] A 3D printing polyurethane material comprises the following components in parts by weight:

[0107] 100 parts of thermoplastic polyurethane elastomer; 7 parts of polyimide / graphene gel powder; 3 parts of zinc stearate.

[0108] Comparative Example 2

[0109] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0110] (1) Graphene oxide, a reducing agent and polyethylene glycol PEG800 are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and placed in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol PEG800 is 1:0.2; the graphene oxide concentration in the graphene oxide mixed solution is 1.2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 h;

[0111] (2) dispersing a diamine monomer and a dianhydride monomer as raw materials in N,N-dimethylformamide to carry out a polycondensation reaction to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.01; the dianhydride monomer is 4,4'-biphenyl ether dianhydride, and the diamine monomer is 4,4'-diaminodiphenylmethane;

[0112] (3) dispersing polyamic acid powder in deionized water, adding tertiary amine triethylamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.4; the mass ratio of graphene oxide to polyamic acid powder is 1:0.5;

[0113] (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel;

[0114] (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0115] A 3D printing polyurethane material comprises the following components in parts by weight:

[0116] 100 parts of thermoplastic polyurethane elastomer; 7 parts of polyimide / graphene gel powder; 3 parts of zinc stearate.

[0117] Comparative Example 3

[0118] A method for preparing polyimide / graphene gel powder comprises the following steps:

[0119] (1) dispersing a diamine monomer and a dianhydride monomer as raw materials in N,N-dimethylformamide for polycondensation to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; the molar ratio of the dianhydride monomer to the diamine monomer is 1:1.01; the dianhydride monomer is 4,4'-biphenyl ether dianhydride, and the diamine monomer is 4,4'-diaminodiphenylmethane;

[0120] (2) dispersing polyamic acid powder in deionized water, adding tertiary amine triethylamine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of polyamic acid powder to tertiary amine is 1:0.4; the mass ratio of graphene oxide to polyamic acid powder is 1:0.5;

[0121] (3) Graphene oxide, a reducing agent, polyethylene glycol PEG800, and a polyamic acid salt solution are dispersed in deionized water to obtain a graphene oxide mixed solution, which is sealed and placed in an oven for heating to obtain a polyamic acid / graphene mixed hydrogel; the mass ratio of graphene oxide to polyethylene glycol PEG800 is 1:0.05; the concentration of graphene oxide in the graphene oxide mixed solution is 1.2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 h;

[0122] (4) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

[0123] A 3D printing polyurethane material comprises the following components in parts by weight:

[0124] 100 parts of thermoplastic polyurethane elastomer; 7 parts of polyimide / graphene gel powder; 3 parts of zinc stearate.

[0125] The polyurethane materials in Examples 1-7 and Comparative Examples 1-3 were printed into strips, and the tensile properties of the strips were tested with reference to GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber, and their electromagnetic shielding properties were tested using a shielding effectiveness meter.

[0126]

[0127] Figure 1 This is a scanning electron microscope image of the polyimide / graphene gel powder prepared in Example 5. It can be seen from the figure that polyethylene glycol, as a good modifier, is not only beneficial to the dispersion of graphene, but also can enhance the interaction force between graphene sheets and improve the stability of the graphene hydrogel structure. The graphene sheet structure of the prepared polyimide / graphene gel powder is connected by filaments formed by polyimide, with small pores and increased porosity, which improves the stability of the gel structure and is beneficial to the improvement of the tensile strength and shielding performance of the 3D printed polyurethane material. Figure 2 This is a scanning electron microscope image of the polyimide / graphene gel powder prepared in Comparative Example 1; due to the lack of polyethylene glycol, the graphene sheet structure is no longer clear, and agglomeration occurs between graphene and between graphene and polyimide. The pores are larger and the porosity is reduced, which is not conducive to multiple reflections and absorption of electromagnetic shielding. Figure 3-4The X-band electromagnetic shielding performance diagram of 3D printed polyurethane materials prepared in Examples 1-7 and Comparative Examples 1-3, combined with Table 1, can be seen that the graphene hydrogel impregnation polyamic acid salt process not only further improves the mechanical properties of the gel material, but also improves the compatibility of graphene and polyurethane thermoplastic materials, which is conducive to meeting the process of 3D printing secondary processing. Impregnating the prepared anisotropic graphene hydrogel with polyamic acid salt can further reduce the pore size and increase the number of pore walls, thereby improving its reflection loss ability and improving the electromagnetic shielding performance. Comparative Example 2 uses too much polyethylene glycol, resulting in a decrease in the porosity of the gel, which is not conducive to the improvement of the electromagnetic shielding performance. Comparative Example 3 is a process for preparing polyimide / graphene gel powder by in-situ polymerization commonly used in the art. Since the gel network is not constructed in advance, the mechanical properties and electromagnetic shielding properties of the gel powder are poor.

[0128] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing polyimide / graphene gel powder, It is characterized in that The following steps are involved: (1) dispersing graphene oxide, a reducing agent and polyethylene glycol in deionized water to obtain a graphene oxide mixed solution, sealing the mixed solution and placing the mixed solution in an oven for heating to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:(0.01-0.1); (2) dispersing a diamine monomer and a dianhydride monomer as raw materials in an organic solvent for polycondensation to prepare a polyamic acid solution; pouring the polyamic acid solution into deionized water for precipitation to obtain a polyamic acid powder; (3) dispersing polyamic acid powder in deionized water, adding tertiary amine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:(0.1-1); (4) under stirring, adding the polyamic acid salt solution dropwise to the graphene hydrogel solution, and after the addition is completed, allowing the solution to stand to obtain a polyamic acid / graphene mixed hydrogel; (5) The polyamic acid / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain polyimide / graphene gel powder.

2. A method for preparing a polyimide / graphene gel powder according to claim 1, It is characterized in that Step (1) The graphene oxide concentration in the graphene oxide mixed solution is 0.5-2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:(0.1-0.5).

3. A method for preparing a polyimide / graphene gel powder according to claim 1, It is characterized in that In step (1), the heating reaction temperature is 60-90° C. and the time is 1-4 h.

4. A method for preparing a polyimide / graphene gel powder according to claim 1, It is characterized in that In step (2), the dianhydride monomer is at least one of 4,4'-biphenyl ether dianhydride, biphenyl tetracarboxylic acid dianhydride, 1,2,4,5-pyromellitic acid dianhydride, 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride, bisphenol A type diether dianhydride, 4,4-oxydiphthalic anhydride, and 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride; the diamine monomer is at least one of p-phenylenediamine, m-phenylenediamine, diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ether, and 4,4'-diaminodiphenylmethane.

5. A method for preparing a polyimide / graphene gel powder according to claim 1, It is characterized in that The organic solvent in step (2) is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and N-methylpyrrolidone.

6. A method for preparing a polyimide / graphene gel powder according to claim 1, It is characterized in that In step (3), the tertiary amine is at least one of triethylamine, tripropylamine and triethanolamine.

7. A method for preparing a polyimide / graphene gel powder according to claim 1, It is characterized in that In step (3), the mass ratio of polyamic acid powder to tertiary amine is 1:(0.3-0.6).

8. A polyimide / graphene gel powder, Features: The polyimide / graphene gel powder is prepared by the preparation method of the polyimide / graphene gel powder according to any one of claims 1 to 7.

9. An application of the polyimide / graphene gel powder as claimed in claim 8, It is characterized in that Polyimide / graphene gel powder is used in the field of 3D printing polyurethane materials.

10. A 3D printing polyurethane material, Features: Contains the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 5-10 parts of polyimide / graphene gel powder; 1-5 parts of flow modifier; the polyimide / graphene gel powder is the polyimide / graphene gel powder according to claim 8.

Citation Information

Patent Citations

  • Method for preparing polyimide-graphene composite aerogel through in-situ polymerization

    CN106750290A

  • Structured carbon aerogel based on 3D printing and preparation method thereof

    CN110357067A

  • Impedance gradient type graphene-based polyimide composite foam wave-absorbing material

    CN112094426A

  • Polyimide-based shape memory composite aerogel and preparation method thereof

    CN116218018A

  • Preparation method of graphene / polyimide-based carbon aerogel

    CN104355302A