A wear-resistant low-smoke halogen-free power cable and a preparation method thereof

By using modified acrylonitrile-butadiene-styrene copolymer and polyvinyl alcohol-modified barite powder in the sheath layer of low-smoke halogen-free power cables, the cable wear resistance and aging resistance are solved. Problem, significantly improving the wear and aging resistance of the cable, extending service life and reducing maintenance costs.

CN118702985BActive Publication Date: 2024-11-22FEIHONG CABLE GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411177971.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-22
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The wear resistance and aging resistance of existing low-smoke halogen-free power cables are poor, and are prone to damage due to mechanical wear and environmental factors, which affects service life and safety performance.

Method used

Using sheath layer combination materials, including linear low density polyethylene, modified acrylonitrile-butadiene-styrene copolymer, polycarbonate, antioxidant, plasticizer and flame retardant, and through barite powder and Bismaleimide modification, combined with polyvinyl alcohol modified barite powder, enhances the binding force of components and improves the wear and aging resistance of the cable.

Benefits of technology

It significantly improves the wear resistance and aging resistance of low-smoke halogen-free power cables, extends service life, reduces maintenance costs, and enhances safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the field of cable technology, and proposes a wear-resistant low-smoke halogen-free power cable and a preparation method thereof. The low-smoke halogen-free power cable comprises a conductor, an insulating layer and a sheath layer from the inside to the outside, and the sheath layer comprises the following components by weight: 40 to 60 parts of linear low-density polyethylene, 25 to 40 parts of acrylonitrile-butadiene-styrene copolymer, 10 to 20 parts of polycarbonate, 1 to 3 parts of antioxidant, 1 to 3 parts of plasticizer, and 15 to 25 parts of flame retardant. Through the above technical scheme, the problems of poor wear resistance and poor aging resistance of low-smoke halogen-free power cables in related technologies are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cables, and in particular to a wear-resistant low-smoke halogen-free power cable and a preparation method thereof. Background Art

[0002] Low smoke halogen-free power cable is a cable with special properties. Its main feature is that it produces less smoke when burning and does not contain halogen. This low smoke characteristic can reduce smoke emissions when a fire occurs, thereby improving the visibility of the fire scene and providing better conditions for personnel evacuation and fire rescue. Halogen-free means that the cable will not release halogen-containing toxic gases such as hydrogen chloride and hydrogen bromide during the combustion process, reducing the harm to the human body and the environment. Although the current low smoke halogen-free power cable has good low smoke characteristics and flame retardancy, it has advantages in environmental protection and safety, but its wear resistance and aging resistance are not outstanding. When the low smoke halogen-free power cable is subjected to some mechanical wear, such as dragging, friction, etc., it will cause the outer sheath to be damaged, thereby affecting its service life and safety performance. In addition, the low smoke halogen-free power cable will be affected by various factors such as temperature, humidity, and light during use, which will accelerate its aging process and cannot meet the needs of long-term stable operation. Therefore, the development of a low smoke halogen-free power cable with good wear resistance and aging resistance plays an important role in reducing its maintenance cost and improving its operating efficiency. Summary of the invention

[0003] The present invention provides a wear-resistant low-smoke halogen-free power cable and a preparation method thereof, which solves the problem of poor wear resistance and poor aging resistance of the low-smoke halogen-free power cable in the related art.

[0004] The technical solution of the present invention is as follows:

[0005] The present invention provides a wear-resistant low-smoke halogen-free power cable, which comprises a conductor, an insulating layer and a sheath layer from the inside to the outside, wherein the sheath layer comprises the following components in parts by weight:

[0006] 40-60 parts of linear low-density polyethylene, 25-40 parts of acrylonitrile-butadiene-styrene copolymer, 10-20 parts of polycarbonate, 1-3 parts of antioxidant, 1-3 parts of plasticizer, and 15-25 parts of flame retardant.

[0007] As a further technical solution, the acrylonitrile-butadiene-styrene copolymer is a modified acrylonitrile-butadiene-styrene copolymer, and the modified acrylonitrile-butadiene-styrene copolymer is obtained by modifying the acrylonitrile-butadiene-styrene copolymer with barite powder and bismaleimide.

[0008] When the acrylonitrile-butadiene-styrene copolymer is a modified acrylonitrile-butadiene-styrene copolymer, it is modified by using barite powder and bismaleimide to improve the toughness of the acrylonitrile-butadiene-styrene copolymer and strengthen the effective combination with the components in the sheath layer, thereby further improving the wear resistance and aging resistance of the low-smoke halogen-free power cable.

[0009] As a further technical solution, the weight ratio of the acrylonitrile-butadiene-styrene copolymer, barite powder and bismaleimide is 7-17:2.5:0.5.

[0010] When the weight ratio of acrylonitrile-butadiene-styrene copolymer, barite powder and bismaleimide is 7~17:2.5:0.5, the wear resistance and aging resistance of the low-smoke halogen-free power cable can be further improved.

[0011] As a further technical solution, the preparation method of the modified acrylonitrile-butadiene-styrene copolymer comprises the following steps: blending acrylonitrile-butadiene-styrene copolymer, barite powder and bismaleimide to obtain the modified acrylonitrile-butadiene-styrene copolymer.

[0012] As a further technical solution, during the blending, the temperature is 145-155° C. and the time is 25-45 min.

[0013] As a further technical solution, the barite powder is polyvinyl alcohol modified barite powder.

[0014] The surface modification of barite powder with polyvinyl alcohol can not only improve the dispersibility of barite powder, but also promote the effective combination of barite powder and acrylonitrile-butadiene-styrene copolymer, and further improve the wear resistance and aging resistance of low-smoke halogen-free power cables.

[0015] As a further technical solution, the preparation method of the polyvinyl alcohol modified barite powder includes the following steps: dissolving polyvinyl alcohol in water to obtain a polyvinyl alcohol solution, adding barite powder to the polyvinyl alcohol solution, stirring, concentrating and drying to obtain the polyvinyl alcohol modified barite powder.

[0016] As a further technical solution, the weight ratio of the barite powder to the polyvinyl alcohol is 4~9:1.

[0017] When the weight ratio of barite powder to polyvinyl alcohol is 4~9:1, the wear resistance and aging resistance of the low-smoke halogen-free power cable can be further improved.

[0018] As a further technical solution, the antioxidant is one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168; the plasticizer is one or more of dioctyl phthalate, epoxy fatty acid methyl ester, and diisononyl phthalate; and the flame retardant is one or both of magnesium hydroxide and aluminum hydroxide.

[0019] As a further technical solution, the mass fraction of the polyvinyl alcohol solution is 5% to 8%.

[0020] The present invention also proposes a method for preparing the wear-resistant low-smoke halogen-free power cable, comprising the following steps:

[0021] S1, mixing the components of the sheath layer to obtain a sheath layer material;

[0022] S2, coating the insulating layer on the surface of the conductor to obtain a conductor with an insulating layer on the surface;

[0023] S3. Covering the sheath layer material on the surface of the conductor having an insulating layer on the outside to obtain the low-smoke halogen-free power cable.

[0024] As a further technical solution, in step S1, during the mixing, the temperature is 140-155° C. and the time is 30-60 min.

[0025] The working principle and beneficial effects of the present invention are:

[0026] In the present invention, the sheath layer uses linear low-density polyethylene as a matrix, and acrylonitrile-butadiene-styrene copolymer is added. The acrylonitrile-butadiene-styrene copolymer can be effectively combined with the polycarbonate in the sheath layer, which can strengthen the internal function of the sheath layer, thereby helping to improve the overall stability of the sheath layer, thereby improving the wear resistance and aging resistance of the low-smoke halogen-free power cable. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the following examples and comparative examples, the model of linear low-density polyethylene is DFDA-7540; the model of acrylonitrile-butadiene-styrene copolymer is PA-765; the model of polycarbonate is RX3440; the particle size of barite powder is 325 mesh; and the model of polyvinyl alcohol is PVA 1799H.

[0029] Example 1

[0030] A wear-resistant low-smoke halogen-free power cable comprises a conductor, an insulating layer and a sheath layer from the inside to the outside, wherein the sheath layer comprises the following components in parts by weight:

[0031] 40 parts of linear low density polyethylene, 25 parts of acrylonitrile-butadiene-styrene copolymer, 10 parts of polycarbonate, 1 part of antioxidant 1076, 1 part of diisononyl phthalate, 15 parts of magnesium hydroxide;

[0032] The preparation method thereof comprises the following steps:

[0033] S1, mixing the components of the sheath layer at 140° C. for 60 min to obtain a sheath layer material;

[0034] S2, coating the insulating layer on the surface of the conductor to obtain a conductor with an insulating layer on the surface;

[0035] S3. Wrap the sheath layer material on the surface of the conductor with an insulating layer to obtain a low-smoke halogen-free power cable.

[0036] Example 2

[0037] A wear-resistant low-smoke halogen-free power cable comprises a conductor, an insulating layer and a sheath layer from the inside to the outside, wherein the sheath layer comprises the following components in parts by weight:

[0038] 50 parts of linear low density polyethylene, 30 parts of acrylonitrile-butadiene-styrene copolymer, 15 parts of polycarbonate, 2 parts of antioxidant 1076, 2 parts of diisononyl phthalate, 20 parts of magnesium hydroxide;

[0039] The preparation method thereof comprises the following steps:

[0040] S1, mixing the components of the sheath layer at 145° C. for 40 min to obtain a sheath layer material;

[0041] S2, coating the insulating layer on the surface of the conductor to obtain a conductor with an insulating layer on the surface;

[0042] S3. Wrap the sheath layer material on the surface of the conductor with an insulating layer to obtain a low-smoke halogen-free power cable.

[0043] Example 3

[0044] A wear-resistant low-smoke halogen-free power cable comprises a conductor, an insulating layer and a sheath layer from the inside to the outside, wherein the sheath layer comprises the following components in parts by weight:

[0045] 60 parts of linear low density polyethylene, 40 parts of acrylonitrile-butadiene-styrene copolymer, 20 parts of polycarbonate, 3 parts of antioxidant 1076, 3 parts of diisononyl phthalate, 25 parts of magnesium hydroxide;

[0046] The preparation method thereof comprises the following steps:

[0047] S1, mixing the components of the sheath layer at 155° C. for 30 min to obtain a sheath layer material;

[0048] S2, coating the insulating layer on the surface of the conductor to obtain a conductor with an insulating layer on the surface;

[0049] S3. Wrap the sheath layer material on the surface of the conductor with an insulating layer to obtain a low-smoke halogen-free power cable.

[0050] Example 4

[0051] The only difference between this embodiment and embodiment 3 is that the acrylonitrile-butadiene-styrene copolymer is a modified acrylonitrile-butadiene-styrene copolymer, and the modified acrylonitrile-butadiene-styrene copolymer is obtained by modifying the acrylonitrile-butadiene-styrene copolymer with barite powder and bismaleimide, and its preparation method comprises the following steps: 25 parts of acrylonitrile-butadiene-styrene copolymer, 12.5 parts of barite powder and 2.5 parts of bismaleimide are blended at 150° C. for 40 minutes to obtain a modified acrylonitrile-butadiene-styrene copolymer.

[0052] Example 5

[0053] The only difference between this embodiment and embodiment 4 is that 37 parts of acrylonitrile-butadiene-styrene copolymer, 2.5 parts of barite powder and 0.5 parts of bismaleimide are added.

[0054] Example 6

[0055] The only difference between this embodiment and embodiment 4 is that 34 parts of acrylonitrile-butadiene-styrene copolymer, 5 parts of barite powder and 1 part of bismaleimide are added.

[0056] Example 7

[0057] The only difference between this embodiment and embodiment 4 is that 28 parts of acrylonitrile-butadiene-styrene copolymer, 10 parts of barite powder and 2 parts of bismaleimide are added.

[0058] Example 8

[0059] The difference between this embodiment and embodiment 5 is that barite powder is not added and 9 parts of bismaleimide are added.

[0060] Example 9

[0061] The difference between this embodiment and embodiment 5 is that bismaleimide is not added and 9 parts of barite powder are added.

[0062] Example 10

[0063] The only difference between this embodiment and Embodiment 7 is that the barite powder is polyvinyl alcohol modified barite powder, and its preparation method comprises the following steps: dissolving 3 parts of polyvinyl alcohol in water to obtain a polyvinyl alcohol solution with a mass fraction of 5%, adding 7 parts of barite powder to the polyvinyl alcohol solution with a mass fraction of 5%, stirring, concentrating and drying to obtain polyvinyl alcohol modified barite powder.

[0064] Embodiment 11

[0065] The only difference between this embodiment and embodiment 10 is that 9.5 parts of barite powder and 0.5 parts of polyvinyl alcohol are added.

[0066] Example 12

[0067] The only difference between this embodiment and embodiment 10 is that 8 parts of barite powder and 2 parts of polyvinyl alcohol are added.

[0068] Example 13

[0069] The only difference between this embodiment and embodiment 10 is that 9 parts of barite powder and 1 part of polyvinyl alcohol are added.

[0070] Comparative Example 1

[0071] The only difference between this comparative example and Example 1 is that no acrylonitrile-butadiene-styrene copolymer is added, and 65 parts of linear low-density polyethylene are added.

[0072] The sheath layer materials of the low-smoke halogen-free power cables prepared by the preparation methods of Examples 1 to 13 and Comparative Example 1 were subjected to the following performance tests:

[0073] Wear resistance: According to GB / T 3960-2016 "Plastic sliding friction and wear test method", the wear resistance of the sheath material of the low-smoke halogen-free power cable is tested;

[0074] Aging resistance: The tensile strength of the sheath material of the low-smoke halogen-free power cable before the aging test was determined according to GB / T 1040.1-2018 "Determination of tensile properties of plastics Part 1: General Principles", wherein the test speed was 200 mm / min; after the aging test was carried out according to GB / T 7141-2008 "Test method for thermal aging of plastics", the tensile strength after the aging test was measured according to the above tensile strength test method, and the aging tensile strength retention rate was calculated according to the following formula: aging tensile strength retention rate = tensile strength after aging test / tensile strength before aging test × 100%; wherein, when the aging test was carried out, the ventilation rate was 50 times / h, the experimental temperature was 90°C, and the exposure time was 128h; 5 samples were taken from each embodiment and comparative example to carry out tensile strength tests before and after the aging test, and the average value of the 5 samples was taken as the result value;

[0075] The test results are shown in Table 1 below:

[0076] Table 1 Test results

[0077]

[0078] Compared with Comparative Example 1, the wear amount of Example 1 is significantly reduced, and the tensile strength before the aging test and the aging tensile strength retention rate are significantly improved, indicating that the addition of acrylonitrile-butadiene-styrene copolymer in the sheath layer can improve the wear resistance and aging resistance of the low-smoke halogen-free power cable.

[0079] Compared with Examples 3 and 8-9, the wear amount of Examples 4-7 is reduced, and the tensile strength before the aging test and the retention rate of the tensile strength against aging are improved, indicating that the use of barite powder and bismaleimide to modify acrylonitrile-butadiene-styrene copolymer can improve the wear resistance and aging resistance of low-smoke halogen-free power cables. Compared with Examples 4-5, the wear amount of Examples 6-7 is reduced, and the tensile strength before the aging test and the retention rate of the tensile strength against aging are improved, indicating that when the weight ratio of acrylonitrile-butadiene-styrene copolymer, barite powder and bismaleimide is 7-17:2.5:0.5, the wear resistance and aging resistance of low-smoke halogen-free power cables can be further improved. Compared with Example 7, the wear amount of Examples 10-13 is reduced, and the tensile strength before the aging test and the retention rate of the tensile strength against aging are improved, indicating that the use of polyvinyl alcohol to modify the surface of barite powder can further improve the wear resistance and aging resistance of low-smoke halogen-free power cables. Compared with Examples 10 to 11, the wear amount of Examples 12 to 13 is reduced, and the tensile strength before the aging test and the aging tensile strength retention rate are improved, indicating that when the weight ratio of barite powder to polyvinyl alcohol is 4 to 9:1, the wear resistance and aging resistance of the low-smoke halogen-free power cable can be further improved.

[0080] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A wear-resistant low-smoke halogen-free power cable, comprising a conductor, an insulation layer and a sheath layer from the inside to the outside, characterized in that: The sheath layer comprises the following components in parts by weight: 40-60 parts of linear low-density polyethylene, 25-40 parts of acrylonitrile-butadiene-styrene copolymer, 10-20 parts of polycarbonate, 1-3 parts of antioxidant, 1-3 parts of plasticizer, 15-25 parts of flame retardant; The acrylonitrile-butadiene-styrene copolymer is a modified acrylonitrile-butadiene-styrene copolymer, and the modified acrylonitrile-butadiene-styrene copolymer is obtained by modifying acrylonitrile-butadiene-styrene copolymer with barite powder and bismaleimide; The preparation method of the modified acrylonitrile-butadiene-styrene copolymer comprises the following steps: blending acrylonitrile-butadiene-styrene copolymer, barite powder and bismaleimide to obtain the modified acrylonitrile-butadiene-styrene copolymer.

2. The wear-resistant low-smoke halogen-free power cable according to claim 1, characterized in that: The weight ratio of the acrylonitrile-butadiene-styrene copolymer, barite powder and bismaleimide is 7-17:2.5:0.

5.

3. The wear-resistant low-smoke halogen-free power cable according to claim 1, characterized in that: The barite powder is polyvinyl alcohol modified barite powder.

4. The wear-resistant low-smoke halogen-free power cable according to claim 3, characterized in that: The preparation method of the polyvinyl alcohol modified barite powder comprises the following steps: dissolving polyvinyl alcohol in water to obtain a polyvinyl alcohol solution, adding barite powder to the polyvinyl alcohol solution, stirring, concentrating and drying to obtain the polyvinyl alcohol modified barite powder.

5. The wear-resistant low-smoke halogen-free power cable according to claim 4, characterized in that: The weight ratio of the barite powder to the polyvinyl alcohol is 4-9:

1.

6. The wear-resistant low-smoke halogen-free power cable according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168; the plasticizer is one or more of dioctyl phthalate, epoxy fatty acid methyl ester, and diisononyl phthalate; and the flame retardant is one or both of magnesium hydroxide and aluminum hydroxide.

7. A method for preparing a wear-resistant low-smoke halogen-free power cable according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, mixing the components of the sheath layer to obtain a sheath layer material; S2, coating the insulating layer on the surface of the conductor to obtain a conductor with an insulating layer on the surface; S3. Covering the sheath layer material on the surface of the conductor having an insulating layer on the outside to obtain the low-smoke halogen-free power cable.

8. The method for preparing a wear-resistant low-smoke halogen-free power cable according to claim 7, characterized in that: In step S1, during the mixing, the temperature is 140-155° C. and the time is 30-60 min.