A composite flame retardant material and preparation method thereof
By using polysiloxane-coated ammonium polyphosphate and nanoferrous trioxide flame retardant in polyvinyl chloride materials, the problem of insufficient flame retardant performance of traditional materials is solved, and efficient flame retardant effect and mechanical performance improvement are achieved , significantly improves the safety of the fire scene.
Patent Information
- Application Number
- CN202411189329.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-28
AI Technical Summary
Traditional polyvinyl chloride materials lack flame retardant properties. The use of a large amount of halogen flame retardant will produce harmful gases and drips, affecting the safety of the fire site. Inorganic flame retardant needs to be added in large quantities to achieve flame retardant effects and affect the mechanical properties of the material.
Polysiloxane coated with ammonium polyphosphate and nanoferric oxide as flame retardant, and the compatibility and stability of flame retardant are improved through microencapsulation and packaging, and in polyvinyl chloride, polylactic acid and Polyurethane compounding is added to improve the flame retardant properties of the material.
It achieves efficient flame retardant performance, with the ultimate oxygen index reaching 34.6-39.5%, and the UL-94 fire resistance level reaches V-0, reducing the risk of flue gas generation and fire spread during combustion of the material, improving the mechanical properties and fire safety of the material .
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer materials, and in particular to a composite flame retardant material and a preparation method thereof. Background Art
[0002] Polyvinyl chloride (PVC) is the third largest synthetic polymer plastic in the world. There are two types of PVC: hard and soft. Hard PVC is used for building pipes, doors and windows, etc. Adding plasticizers can make PVC softer, more elastic and ductile. It can be used for cable insulation, the surface of saddle leather covers, etc.
[0003] During the production process of saddles, the leather covers of the saddles are usually piled up in the workshop. If they accidentally come into contact with a fire source, they are likely to burn and cause a fire.
[0004] Conventional common PVC materials have no flame retardant properties and will burn quickly when encountering flames. In order to make PVC materials have good flame retardant properties, a large amount of halogen compounds (decabromodiphenylethane, brominated polystyrene, etc.) are added to the materials in general processes. Although the flame retardant effect is improved, a large amount of halogen harmful gases will be produced in the fire. Most of the victims at the fire scene are actually killed by the thick smoke and toxic substances in the thick smoke. Studies have shown that HC50 concentration / PPM3800 gas concentration can cause fatal coma of escapees; at the same time, the material will produce a large amount of burning drippings during the combustion process, causing the spread of the fire and expanding the fire situation.
[0005] In order to avoid the harm of halogen, inorganic flame retardants (oxides, hydroxides) are used to replace halogen flame retardants. However, although inorganic flame retardants have overcome many defects of halogen flame retardants, they need to be added in large quantities to achieve flame retardant effects, which seriously affects the mechanical properties of polyvinyl chloride materials, especially polyvinyl chloride films. Summary of the invention
[0006] In order to improve the flame retardant properties of a material while ensuring the mechanical properties of the material, the present application provides a composite flame retardant material and a preparation method thereof.
[0007] In a first aspect, the present application provides a composite flame retardant material, which adopts the following technical solution:
[0008] A composite flame retardant material, comprising the following raw materials in parts by weight: 100-120 parts of polyvinyl chloride, 15-30 parts of polylactic acid, 20-40 parts of polyurethane, 10-15 parts of flame retardant, 1-2 parts of antioxidant, and 10-30 parts of plasticizer;
[0009] The flame retardant is made of polysiloxane-coated ammonium polyphosphate and nano-iron trioxide;
[0010] The weight ratio of the ammonium polyphosphate to the nano-ferric oxide is (50-60):1.
[0011] By adopting the above technical solution, polyvinyl chloride, polylactic acid and polyurethane are compounded as the matrix. Both polyvinyl chloride and polyurethane have high strength and toughness, and can provide good mechanical support for the film. Both polylactic acid and polyurethane have good plastic processing and molding capabilities, making the compound film easy to process and mold. The three are compounded in a suitable ratio to obtain a film material with better comprehensive performance.
[0012] Adding polysiloxane to the resin matrix to encapsulate ammonium polyphosphate and nano-ferric oxide to make a flame retardant, ammonium polyphosphate as a flame retardant, while providing acid source and gas source, can effectively inhibit the generation of smoke when the polymer burns, which is in line with the trend of green, environmental protection, smoke suppression, and high-efficiency flame retardancy. However, when ammonium polyphosphate is added to the matrix of polyvinyl chloride, polylactic acid and polyurethane, it has poor compatibility and is easy to absorb moisture in the air, which then migrates to the surface of the material and causes loss, resulting in reduced mechanical properties and flame retardant efficiency of the polymer film. Ammonium polyphosphate is microencapsulated with polysiloxane, which contains Si-O-Si bonds, and the Si-O bond length is relatively long, the Si-O-Si bond angle is large, and the bond energy is much greater than the CC bond and CO bond energy in the polymer material. After ammonium polyphosphate is microencapsulated by polysiloxane, the Si-O-Si bond in silicone can be grafted onto the surface of ammonium polyphosphate to improve the hydrophobicity, thermal stability and compatibility of ammonium polyphosphate with the matrix, which plays an important role in improving the flame retardant properties of the film.
[0013] Nano ferric oxide is used as a synergist and is wrapped in a polysiloxane capsule together with ammonium polyphosphate. Nano ferric oxide and ammonium polyphosphate have excellent synergistic flame retardant effects. Ammonium polyphosphate improves the flame retardant and smoke suppression properties of the matrix. Nano ferric oxide has excellent carbonization promotion effect, which is conducive to the formation of a more thermally stable expanded carbon layer in the matrix during pyrolysis to block heat and mass transfer, improve the density of the carbon layer of the matrix material, make up for the defect of the non-dense carbon layer structure of ammonium polyphosphate, and improve the flame retardant efficiency. In addition, nano ferric oxide is wrapped in a polysiloxane capsule, which solves the problem that nano ferric oxide is easy to agglomerate in the matrix.
[0014] The synergistic effect of polysiloxane, ammonium polyphosphate and nano-ferric oxide improves the flame retardant properties of the material. The limiting oxygen index of the obtained film material can reach 34.6-39.5%, and the UL-94 fire rating can reach V-0. Using a film with high flame retardant properties as the surface of the saddle leather cover improves the flame retardant properties of the saddle leather cover, reduces the probability of accumulated leather covers burning in the workshop and causing fires, and improves the fire safety of the production workshop.
[0015] Furthermore, the preparation method of the flame retardant is:
[0016] 1) Disperse ammonium polyphosphate and nano-ferric oxide in a dispersion to obtain a mixed solution, and add a pH regulator to adjust the pH value of the mixed solution to 9-11;
[0017] 2) Add siloxane and tetraethyl orthosilicate to the above mixed solution and react at 40-50°C for 2-3h; after the reaction, filter to obtain a precipitate, wash and extract the precipitate, and then dry it to obtain a flame retardant.
[0018] By adopting the above technical scheme, ammonium polyphosphate and nano-ferric oxide are mixed as the core material, siloxane and tetraethyl orthosilicate are used as precursors, and the core material is microencapsulated and coated by the sol-gel process to obtain a flame retardant. On the one hand, ammonium polyphosphate and nano-ferric oxide can be in closer contact, so that nano-ferric oxide can fully exert its synergistic effect on ammonium polyphosphate, improve the stability and density of the carbon layer formed during the pyrolysis of the matrix, and improve the flame retardant efficiency; on the other hand, the polysiloxane capsule can simultaneously improve the compatibility of ammonium polyphosphate and nano-ferric oxide with the matrix, ensure the stable existence of the flame retardant in the matrix, and give full play to its flame retardant effect.
[0019] Furthermore, the flame retardant also includes a lipid material, and the lipid material is added into the mixed solution along with siloxane and tetraethyl orthosilicate.
[0020] By adopting the above technical solution, lipid materials are added to the wall material of the microcapsule. As a component of the microcapsule, the lipid materials can provide a carbon source and improve the flame retardant effect of the flame retardant. In addition, the addition of lipid materials can also improve the stability of the microcapsule.
[0021] Furthermore, the lipid material includes one or more of fatty acids and phospholipids.
[0022] Furthermore, the weight ratio of siloxane: tetraethyl orthosilicate: lipid material is (5-7): (6-8): 1.
[0023] Furthermore, the siloxane includes one or more of dimethyldiethoxysilane, methyltriethoxysilane, and phenyltrimethoxysilane.
[0024] Furthermore, the siloxane comprises dimethyldiethoxysilane and methyltriethoxysilane in a weight ratio of (2-5):1.
[0025] Furthermore, the particle size of the nano-iron oxide is 10-30 nm.
[0026] Furthermore, it also includes hexadecyl phase change microcapsules.
[0027] Furthermore, the weight ratio of the n-hexadecyl phase change microcapsules to the flame retardant is 1:(2-4).
[0028] By adopting the above technical scheme, the addition of n-hexadecyl phase change microcapsules can, on the one hand, improve the thermal insulation and heat storage properties of the film and greatly enhance its fire safety; on the other hand, it can synergize with the flame retardant to further enhance the flame retardant effect.
[0029] In a second aspect, the present application provides a method for preparing a composite flame retardant material, comprising the following steps:
[0030] S1. The polyvinyl chloride, polylactic acid, polyurethane, flame retardant, antioxidant, plasticizer and optional hexadecyl phase change microcapsules are mixed and mixed to obtain a mixing material;
[0031] S2. Extruding the mixed material to obtain a composite flame retardant material.
[0032] By adopting the above technical solution, the preparation method of the present application is simple and easy to operate, has no special requirements for production equipment, and is suitable for industrial production.
[0033] In summary, this application has the following beneficial effects:
[0034] Ammonium polyphosphate and nano-ferric oxide are microencapsulated with polysiloxane to obtain a flame retardant, which is added to the resin matrix to prepare a flame retardant material, which can be evenly dispersed in the resin matrix. Ammonium polyphosphate provides both an acid source and a gas source, which can effectively suppress the generation of smoke when the polymer burns, and is in line with the trend of green, environmentally friendly, smoke-suppressing, and efficient flame retardancy. As a synergist, nano-ferric oxide has an excellent synergistic flame retardant effect with ammonium polyphosphate. Nano-ferric oxide has an excellent carbonization-promoting effect, which is beneficial to the formation of a more thermally stable expanded carbon layer in the matrix during pyrolysis to block heat and mass transfer, improve the density of the carbon layer of the matrix material, make up for the defect of the non-dense carbon layer structure of ammonium polyphosphate, and improve the flame retardant efficiency. The limiting oxygen index of the flame retardant material obtained can reach 34.6-39.5%, and the UL-94 fire rating can reach V-0. DETAILED DESCRIPTION
[0035] The present application is further described in detail below with reference to the embodiments.
[0036] Raw materials and intermediate preparation examples
[0037] raw material
[0038] The raw materials in the examples of this application can be obtained from the market:
[0039] Polyvinyl chloride, S-1000, melt index 1000-1100g / 10min;
[0040] Polylactic acid, PLA 4060D, melt flow rate 3g / 10min;
[0041] Polyurethane, TPU-80A;
[0042] Antioxidant, bisphenol A antioxidant;
[0043] Plasticizer, dioctyl phthalate;
[0044] Ammonium polyphosphate, technical grade;
[0045] Dimethyldiethoxysilane, analytical grade, purity 98%;
[0046] Methyltriethoxysilane, analytical grade, purity 98%;
[0047] Phenyltrimethoxysilane, analytical grade, purity 98%;
[0048] Tetraethyl orthosilicate, analytical grade, purity 98%;
[0049] fatty acid, linoleic acid;
[0050] Hexadecyl phase change microcapsules, phase change temperature 18.1 °C, 5-10 μm particle size, core-shell ratio 7:3, shell material polymethyl methacrylate, were purchased from Hebei Ruosen Technology Co., Ltd.
[0051] Preparation Example
[0052] Preparation Example 1
[0053] A flame retardant, the preparation method of which is:
[0054] 1) 3.2 kg of ammonium polyphosphate and 0.064 kg of nano-ferric oxide were dispersed in 13 L of dispersion liquid (a mixture of anhydrous ethanol and deionized water in a weight ratio of 2:1) to obtain a mixed solution, and then ammonia water was added dropwise as a pH regulator to adjust the pH value of the mixed solution to 10; the particle size of the nano-ferric oxide was 10 nm;
[0055] 2) Add 0.5 kg of dimethyldiethoxysilane and 0.8 kg of tetraethyl orthosilicate to the above mixed solution, stir and react at 45 °C for 2 h, filter and obtain the precipitate after the reaction, wash it with anhydrous ethanol for 3 times, put the powder into a Soxhlet extractor and extract it with anhydrous ethanol for 20 h, and finally place it in an electric blast drying oven at 80 °C and dry it for 24 h to obtain a flame retardant.
[0056] Preparation Example 2
[0057] A flame retardant, the preparation method of which is:
[0058] 1) Same as Preparation Example 1;
[0059] 2) Add 0.7 kg of dimethyldiethoxysilane and 0.6 kg of tetraethyl orthosilicate to the above mixed solution, stir and react at 45 °C for 2 h, filter and obtain the precipitate after the reaction, wash it with anhydrous ethanol for 3 times, then put the powder into a Soxhlet extractor and extract it with anhydrous ethanol for 20 h, finally place it in an electric blast drying oven at 80 °C and dry it for 24 h to obtain a flame retardant.
[0060] Preparation Example 3
[0061] A flame retardant, the preparation method of which is:
[0062] 1) Same as Preparation Example 1;
[0063] 2) Add 0.6 kg of dimethyldiethoxysilane and 0.7 kg of tetraethyl orthosilicate to the above mixed solution, stir and react at 45 °C for 2 h, filter and obtain the precipitate after the reaction, wash it with anhydrous ethanol for 3 times, then put the powder into a Soxhlet extractor and extract it with anhydrous ethanol for 20 h, finally place it in an 80 °C electric blast drying oven and dry it for 24 h to obtain a flame retardant.
[0064] Preparation Example 4
[0065] A flame retardant, the preparation method of which is:
[0066] 1) Same as Preparation Example 1;
[0067] 2) Add 0.4 kg of dimethyldiethoxysilane, 0.2 kg of methyltriethoxysilane and 0.7 kg of tetraethyl orthosilicate to the above mixed solution, stir and react at 45 °C for 2 h, filter and obtain the precipitate after the reaction, wash it with anhydrous ethanol for 3 times, put the powder into a Soxhlet extractor and extract it with anhydrous ethanol for 20 h, and finally place it in an electric blast drying oven at 80 °C and dry it for 24 h to obtain a flame retardant.
[0068] Preparation Example 5
[0069] A flame retardant, the preparation method of which is:
[0070] 1) Same as Preparation Example 1;
[0071] 2) Add 0.5 kg of dimethyldiethoxysilane, 0.1 kg of methyltriethoxysilane and 0.7 kg of tetraethyl orthosilicate to the above mixed solution, stir and react at 45 °C for 2 h, filter and obtain the precipitate after the reaction, wash it with anhydrous ethanol for 3 times, then put the powder into a Soxhlet extractor and extract it with anhydrous ethanol for 20 h, finally put it into an 80 °C electric blast drying oven and dry it for 24 h to obtain a flame retardant.
[0072] Preparation Example 6
[0073] A flame retardant, the preparation method of which is:
[0074] 1) Same as Preparation Example 1;
[0075] 2) Add 0.2 kg of dimethyldiethoxysilane, 0.4 kg of methyltriethoxysilane and 0.7 kg of tetraethyl orthosilicate to the above mixed solution, stir and react at 45 °C for 2 h, filter and obtain the precipitate after the reaction, wash it with anhydrous ethanol for 3 times, then put the powder into a Soxhlet extractor and extract it with anhydrous ethanol for 20 h, finally place it in an electric blast drying oven at 80 °C and dry it for 24 h to obtain a flame retardant.
[0076] Preparation Example 7
[0077] A flame retardant, the preparation method of which is:
[0078] 1) Disperse 3.2 kg of ammonium polyphosphate and 0.053 kg of nano-ferric oxide in 13 L of dispersion liquid (a mixture of anhydrous ethanol and deionized water in a weight ratio of 2:1) to obtain a mixed solution, and then add ammonia water as a pH regulator to adjust the pH value of the mixed solution to 10; the particle size of the nano-ferric oxide is 10 nm;
[0079] 2) Same as Preparation Example 4.
[0080] Preparation Example 8
[0081] A flame retardant, the preparation method of which is:
[0082] 1) Disperse 3.2 kg of ammonium polyphosphate and 0.070 kg of nano-ferric oxide in 13 L of dispersion liquid (a mixture of anhydrous ethanol and deionized water in a weight ratio of 2:1) to obtain a mixed solution, and then add ammonia water as a pH regulator to adjust the pH value of the mixed solution to 10; the particle size of the nano-ferric oxide is 10 nm;
[0083] 2) Same as Preparation Example 4.
[0084] Preparation Example 9
[0085] A flame retardant, the preparation method of which is:
[0086] Different from Preparation Example 7, the particle size of the nano-iron oxide in Preparation Example 9 is 30 nm.
[0087] Preparation Example 10
[0088] A flame retardant, the preparation method of which is:
[0089] 1) 3.2 kg of ammonium polyphosphate and 0.053 kg of nano-ferric oxide were dispersed in 13 L of dispersion liquid (a mixture of anhydrous ethanol and deionized water in a weight ratio of 2:1) to obtain a mixed solution, and then ammonia water was added dropwise as a pH regulator to adjust the pH value of the mixed solution to 10; the particle size of the nano-ferric oxide was 10 nm;
[0090] 2) Add 0.4 kg of dimethyldiethoxysilane, 0.2 kg of methyltriethoxysilane, 0.7 kg of tetraethyl orthosilicate and 0.1 kg of fatty acid to the above mixed solution, stir and react at 45 °C for 2 h, filter and obtain the precipitate after the reaction, wash it with anhydrous ethanol for 3 times, put the powder into a Soxhlet extractor and extract it with anhydrous ethanol for 20 h, and finally place it in an electric blast drying oven at 80 °C and dry it for 24 h to obtain a flame retardant.
[0091] Preparation Example 11
[0092] A flame retardant, the preparation method of which is:
[0093] 1) Disperse 3.2 kg of ammonium polyphosphate in 13 L of dispersion liquid (a mixture of anhydrous ethanol and deionized water in a weight ratio of 2:1) to obtain a mixed solution, and then add ammonia water as a pH adjuster to adjust the pH value of the mixed solution to 10; the particle size of nano-ferric oxide is 10 nm;
[0094] 2) Add 0.5 kg of dimethyldiethoxysilane and 0.8 kg of tetraethyl orthosilicate to the above mixed solution, stir and react at 45 °C for 2 h, filter and obtain the precipitate after the reaction, wash it with anhydrous ethanol for 3 times, then put the powder into a Soxhlet extractor and extract it with anhydrous ethanol for 20 h, finally place it in an electric blast drying oven at 80 °C and dry it for 24 h to obtain a flame retardant.
[0095] Example
[0096] Examples 1-6
[0097] A composite flame retardant material, the preparation method of which is:
[0098] S1. According to the raw material ratio in Table 1, polyvinyl chloride, polylactic acid, polyurethane, flame retardant, antioxidant, plasticizer, and hexadecyl phase change microcapsules were put into a mixer and stirred at a speed of 550 rpm for 5 min, and then transferred to a mixer and mixed at 150 ° C to obtain a mixed material; wherein the flame retardant is from Preparation Example 1;
[0099] S2. The mixed material is put into an extruder and extruded through a die at 175° C. to obtain a composite flame retardant material.
[0100] Table 1 Raw material ratio table of Examples 1-6 (kg)
[0101]
[0102] Embodiment 7-15
[0103] Different from Example 4, the flame retardants in Examples 7-15 are respectively from Preparation Examples 2-10.
[0104] Comparative Example
[0105] Comparative Example 1
[0106] The difference from Example 1 is that the flame retardant in Comparative Example 1 comes from Preparation Example 11.
[0107] Comparative Example 2
[0108] Different from Example 1, the flame retardant in Comparative Example 2 is ammonium polyphosphate.
[0109] Comparative Example 3
[0110] Different from Example 1, the flame retardant in Comparative Example 3 is ammonium polyphosphate and nano-ferric oxide in a weight ratio of 50:1.
[0111] Performance Testing
[0112] The following performance tests were performed on the composite flame retardant materials obtained in the examples and comparative examples. The test results are shown in Table 2.
[0113] Refer to the standard "Determination of combustion behavior of plastics by oxygen index method Part 2: Room temperature test" GB / T 2406.2-2009 to test the limiting oxygen index of the material;
[0114] The UL-94 fire rating of the material is tested with reference to the standard "Horizontal and vertical methods for the determination of the combustion performance of plastics" GB / T 2408-2021;
[0115] The smoke density of the material is tested with reference to the standard "Plastic Smoke Generation Part 2: Single Chamber Test Method for Determination of Smoke Density" GB / T 8323.2-2008.
[0116] Table 2 Performance test results
[0117]
[0118] Combining Examples 1-15 with Comparative Examples 1-3 and Table 2, it can be seen that the limiting oxygen index of the flame retardant materials obtained in Examples 1-15 is higher than that of Comparative Examples 1-3, the smoke density of the flame retardant materials obtained in Examples 1-15 is lower than that of Comparative Examples 1-3, and the UL-94 fire rating of the flame retardant materials in Examples 1-15 can reach V-0, which indicates that the flame retardant material prepared in the present application has good flame retardant properties.
[0119] Combining Example 1 with Comparative Examples 1-3 and Table 2, it can be seen that in Comparative Example 1, ammonium polyphosphate is microencapsulated and modified, but there is no nano-ferric oxide, in Comparative Example 2, unmodified ammonium polyphosphate is used as a flame retardant, and in Comparative Example 3, unmodified ammonium polyphosphate and nano-ferric oxide are compounded as flame retardants. It can be seen that the flame retardant property of the flame retardant material obtained in Example 1 is significantly better than that of Comparative Examples 1-3, which indicates that the flame retardant obtained by compounding nano-ferric oxide with sodium polyphosphate and performing microencapsulation modification can significantly improve the flame retardant property of the flame retardant material. This may be because ammonium polyphosphate, as a flame retardant, provides both acid and gas sources, which can effectively inhibit the generation of smoke during polymer combustion. Nano-ferric oxide and ammonium polyphosphate have excellent synergistic flame retardant effects. Nano-ferric oxide has excellent carbonization-promoting effects, which is beneficial to the formation of a more thermally stable expanded carbon layer in the matrix during pyrolysis to block heat and mass transfer, improve the density of the carbon layer of the matrix material, and make up for the defect of the non-dense carbon layer structure of ammonium polyphosphate, thereby improving the flame retardant effect. Microencapsulation modification, on the one hand, allows ammonium polyphosphate and nano-ferric oxide to be in closer contact, so that nano-ferric oxide can fully exert its synergistic effect on ammonium polyphosphate, improve the stability and density of the carbon layer formed during the pyrolysis of the matrix, and improve the flame retardant efficiency; on the other hand, polysiloxane capsules can simultaneously improve the compatibility of ammonium polyphosphate and nano-ferric oxide with the matrix, ensure the stable existence of the flame retardant in the matrix, and give full play to its flame retardant effect.
[0120] Combining Examples 1-3 and Table 2, it can be seen that the flame retardant properties of the flame retardant materials obtained in Examples 1-3 are all excellent, among which the ratio in Example 2 is better.
[0121] Combining Example 2 with Examples 4-6 and Table 2, it can be seen that the flame retardant properties of the flame retardant materials in Examples 4-6 are better than those in Example 2, which shows that the addition of n-hexadecyl phase change microcapsules can further improve the flame retardant properties of the flame retardant materials. This may be because the addition of n-hexadecyl phase change microcapsules can improve the thermal insulation and heat storage properties of the film, greatly improving its fire safety; on the other hand, it synergizes with the flame retardant to further improve the flame retardant effect. Among them, the addition amount of n-hexadecyl phase change microcapsules in Example 5 is better.
[0122] Combining Example 4 with Examples 7-8 and Table 2, it can be seen that the ratio of siloxane to tetraethyl orthosilicate affects the flame retardant properties of the flame retardant material, and the ratio in Example 8 is better.
[0123] Combining Example 12 with Example 15 and Table 2, it can be seen that the flame retardant performance of the flame retardant material obtained in Example 15 is better than that of Example 12, which shows that adding lipid materials to microcapsules can improve the flame retardant performance of the material. This may be because the lipid material, as a component of the microcapsule, can provide a carbon source and improve the flame retardant effect of the flame retardant. In addition, the addition of lipid materials can also improve the stability of the microcapsules.
[0124] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A composite flame retardant material, characterized in that: The invention comprises the following raw materials in parts by weight: 100-120 parts of polyvinyl chloride, 15-30 parts of polylactic acid, 20-40 parts of polyurethane, 10-15 parts of flame retardant, 1-2 parts of antioxidant and 10-30 parts of plasticizer; The flame retardant is made of polysiloxane-coated ammonium polyphosphate and nano-iron trioxide; The weight ratio of the ammonium polyphosphate to nano-ferric oxide is (50-60):
1.
2. A composite flame retardant material according to claim 1, characterized in that: The preparation method of the flame retardant is: 1) Dispersing ammonium polyphosphate and nano-ferric oxide in a dispersion to obtain a mixed solution, and adding a pH regulator to adjust the pH value of the mixed solution to 9-11; 2) Add siloxane and tetraethyl orthosilicate to the above mixed solution, and react at 40-50° C. for 2-3 hours; after the reaction is completed, filter to obtain a precipitate, wash and extract the precipitate, and then dry it to obtain a flame retardant.
3. A composite flame retardant material according to claim 2, characterized in that: The flame retardant also includes lipid materials, which are added into the mixed solution along with siloxane and tetraethyl orthosilicate.
4. A composite flame retardant material according to claim 3, characterized in that: The weight ratio of the siloxane:tetraethyl orthosilicate:lipid material is (5-7):(6-8):
1.
5. The composite flame retardant material according to claim 2, characterized in that: The siloxane includes one or more of dimethyldiethoxysilane, methyltriethoxysilane, and phenyltrimethoxysilane.
6. A composite flame retardant material according to claim 5, characterized in that: The siloxane includes dimethyldiethoxysilane and methyltriethoxysilane in a weight ratio of (2-5):
1.
7. The composite flame retardant material according to claim 1, characterized in that: The particle size of the nano-iron sesquioxide is 10-30nm.
8. The composite flame retardant material according to claim 1, characterized in that: Also included are n-hexadecyl phase change microcapsules.
9. A composite flame retardant material according to claim 8, characterized in that: The weight ratio of the n-hexadecyl phase change microcapsules to the flame retardant is 1:(2-4).
10. A method for preparing a composite flame retardant material according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. The polyvinyl chloride, polylactic acid, polyurethane, flame retardant, antioxidant, plasticizer and optional hexadecyl phase change microcapsules are mixed and mixed to obtain a mixing material; S2. Extruding the mixed material to obtain a composite flame retardant material.
Citation Information
Patent Citations
Soft polyvinyl chloride composite material with flame retardancy, smoke inhibition performance and good mechanical property and preparation method of soft polyvinyl chloride composite material
CN110218401A
Hyperbranched polysiloxane coated ammonium polyphosphate flame retardant and preparation method thereof
CN110606990A
Low-smoke halogen-free thermoplastic elastomer fire-resistant cable material and production process