Heat-resistant, corrosion-resistant and waterproof epoxy adhesive material and its preparation method and application
Through the composite material of modified epoxy resin and hyperbranched epoxy resin, combined with nano-fillers, the problem of resistance and corrosion resistance of bridge deck pavement materials in areas with temperature differences between day and night is solved, and the low-temperature resistance, high-temperature resistance and chemical stability of the material are improved. properties and enhanced waterproof performance.
Patent Information
- Application Number
- CN202411178547.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The bonding materials of existing bridge deck pavements are easily damaged due to thermal expansion and contraction, cyclic fatigue, shear strength changes and moisture penetration in areas with large temperature differences between day and night, and cannot meet the needs of temperature resistance and corrosion protection.
It uses a composite material of modified epoxy resin and hyperbranched epoxy resin, and forms a stable three-dimensional structure by compounding different bisphenol A-type epoxy resins and adding modified fillers such as nano-silica, nano-lanthanum oxide, and nano-alumina. The network structure improves the material's low temperature resistance, high temperature resistance and chemical stability.
It significantly improves the low-temperature resistance, high-temperature resistance and chemical stability of the bonding material, reduces the risk of corrosion, enhances the waterproof performance, and extends the service life of the material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road materials, and in particular relates to a heat-resistant, corrosion-resistant and waterproof epoxy bonding material and a preparation method and application thereof. Background Art
[0002] The bonding material of the bridge deck pavement is an important component in the bridge deck waterproofing and paving system. Its main function is to provide a good bonding interface between the concrete bridge deck and the asphalt pavement layer, while also playing a waterproofing role, preventing moisture from penetrating into the concrete structure and protecting the bridge structure from water damage.
[0003] In areas with large temperature differences between day and night, the bonding materials of bridge deck pavement will face a series of technical problems, which are mainly due to the physical and chemical effects caused by temperature changes. Specifically, they are: (1) Expansion and contraction: The temperature difference between day and night will cause the pavement layer and the bridge deck to expand and contract. If the thermal expansion coefficient of the bonding material does not match that of the bridge deck or pavement layer, temperature stress may be generated, causing the bonding layer to crack or delaminate. (2) Cyclic fatigue: Under the action of long-term temperature cycles, the bonding material is prone to fatigue failure, which reduces its performance. (3) Shear strength change: Temperature changes can affect the shear strength of the bonding material. For example, some materials may become brittle at low temperatures and may become too soft at high temperatures, thus affecting their shear resistance. (4) Under high temperature conditions, some bonding materials may exhibit creep behavior, that is, gradually deform under constant stress, which may cause deformation and damage to the pavement layer. (5) Moisture penetration: In an environment with large temperature differences, if the waterproof performance of the bonding material is insufficient, moisture may penetrate into the bridge deck through microcracks or other weak points, causing problems such as steel corrosion.
[0004] In order to improve the temperature resistance of bonding materials, existing technologies usually select materials with good temperature adaptability, such as epoxy asphalt, which has good temperature stability, and conduct detailed thermodynamic analysis before construction to ensure that the selected materials can show good temperature resistance under the target environmental conditions. However, when exposed to outdoor environments for a long time, epoxy asphalt will be affected by ultraviolet radiation, oxidation and other factors, resulting in a decrease in material performance. This cannot meet the needs of the existing market.
[0005] Therefore, a new epoxy bonding material is urgently needed. Summary of the invention
[0006] The purpose of the present invention is to provide a heat-resistant, corrosion-resistant and waterproof epoxy bonding material and a preparation method and application thereof.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] A heat-resistant, corrosion-resistant and waterproof epoxy adhesive material, comprising the following components in parts by weight: 5-9 parts of a modified epoxy resin, 3-6 parts of a hyperbranched epoxy resin, 4-6 parts of a curing agent, 0.3-0.5 parts of a dispersant, 0.2-0.6 parts of a defoaming agent and 7-10 parts of a modified filler;
[0009] The preparation method of the modified epoxy resin is as follows: in a nitrogen environment, 650 parts by weight of bisphenol A epoxy resin is heated to 130-135° C., 0.5-0.7 parts by weight of N,N-dimethylbenzylamine is added, and the reaction is carried out by heat preservation for 12-15 hours, and 30-35 parts by weight of N-methylethanolamine and 200-210 parts of azobisisobutyronitrile are continuously added, and the reaction is carried out at 130-135° C. for 6-8 hours, and the reaction is cooled to room temperature to obtain the modified epoxy resin.
[0010] Furthermore, the bisphenol A epoxy resin is a mixture of bisphenol A epoxy resin E44, bisphenol A epoxy resin E51 and bisphenol A epoxy resin SP-144 in a mass ratio of (0.2-0.5): (1.4-1.7): 1. It is purchased from Jinan Baorui Resin Chemical Co., Ltd.
[0011] The temperature difference between day and night will cause the pavement layer and the bridge deck to produce thermal expansion and contraction, and the adhesive material is prone to breakage. In the prior art, bisphenol A epoxy resin is usually directly used as the main raw material of the adhesive material, but the prepared adhesive material is prone to cracking at low temperatures. The present invention modifies the three bisphenol A epoxy resins after compounding, thereby improving the low temperature resistance of the adhesive material. By mixing epoxy resins with different epoxy values and molecular weights, the flexibility of the final product can be improved, which is beneficial to improving the low temperature resistance; N-methylethanolamine can react with epoxy groups to form a cross-linked structure, and azobisisobutyronitrile decomposes to produce free radicals, thereby inducing a cross-linking reaction, forming a more stable three-dimensional network structure, and enhancing the flexibility and low temperature resistance of the adhesive material. However, the high temperature resistance of the adhesive material is not ideal.
[0012] Furthermore, the preparation method of the hyperbranched epoxy resin is as follows: under nitrogen protection, 180 parts by mass of glycidyl ether and 9.2-9.7 parts by mass of tetrabutylammonium bromide are mixed, heated to 100-110°C, 10-12 parts by mass of a trivalent hydroxy compound are added, stirred for 2-3h, and 10-12 parts by mass of the trivalent hydroxy compound are continued to be added. After the addition is completed, the mixture is reacted at 100-110°C for 10-12h. After the reaction is completed, the mixture is cooled to room temperature, 90-95 parts by mass of tetrahydrofuran are added to dissolve the product, and then the product is precipitated with ethanol for 3-4 times, and dried at 95-100°C under vacuum for 10-15h to obtain a hyperbranched epoxy resin.
[0013] Furthermore, the glycidyl ether is a mixture of 1,2-cyclohexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether and propylene glycol triglycidyl ether in a mass ratio of (0.5-0.8):1:(1.3-1.6).
[0014] Furthermore, the trivalent hydroxy compound is a mixture of trimethylolethane, trimethylolpropane and pentaerythritol in a mass ratio of 1: (1.2-1.5): (0.4-0.7).
[0015] The invention improves the high temperature resistance of the bonding material by adding a hyperbranched epoxy resin and synergizing with a modified epoxy resin. The invention forms a complex branched structure by reacting a glycidyl ether and a trivalent hydroxy compound of a specific type and ratio, and forms a more compact network structure by compounding with the modified epoxy resin. The hyperbranched structure increases the glass transition temperature of the resin, and can still maintain performance at a higher temperature, thereby improving the high temperature resistance of the bonding material. At the same time, the mechanical properties of the bonding material are improved.
[0016] Furthermore, the preparation method of the modified filler is:
[0017] (1) Mixing nano silicon dioxide, nano lanthanum oxide and nano aluminum oxide in a mass ratio of 1: (0.4-0.6): (1.3-1.6) to obtain a mixed filler;
[0018] (2) Mixing a mixed filler in a mass ratio of 1: (0.1-0.15): (10-15), a silane coupling agent KH550 and an ethanol aqueous solution with a mass fraction of 60-70%, stirring at 40-45° C. for 1-2 hours, filtering, and drying to obtain a silane-modified filler;
[0019] (3) Immerse 1 part by mass of the silane-modified filler in 8-10 parts by mass of the treatment liquid, treat it ultrasonically for 1-2 hours, filter it out, and then put it into a plasma irradiator. The irradiation power is 200-300W for plasma irradiation treatment for 20-30 minutes, and then take it out to obtain a modified filler.
[0020] Furthermore, the treatment liquid includes the following components in parts by weight: 12-14 parts of hexadecyltrimethylammonium bromide, 6-9 parts of sodium hexametaphosphate, 10-13 parts of nonylphenol polyoxyethylene ether (NP-10), 7-10 parts of nano-zirconium boride (Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model: ZT-BZr50), and 200 parts of water.
[0021] Furthermore, the nano-silicon dioxide has an average particle size of 20 nm and a specific surface area of 180 ± 50 m 2 / g.
[0022] Furthermore, the particle size of nano-lanthanum oxide is 30nm-50nm, and the specific surface area is 30-50m 2 / g.
[0023] Furthermore, the average particle size of nano-alumina is 0.3 μm, and the specific surface area is 5-10 m 2 / g.
[0024] Gasoline or kerosene leakage may occur during transportation of automobiles, and if not handled in time, it may cause damage to the bridge deck. The present invention can improve the chemical corrosion resistance of the connecting material by adding modified fillers to the bonding material. By modifying the mixed filler, the combination of nano-silicon dioxide, nano-lanthanum oxide and nano-aluminum oxide can improve the chemical resistance of the composite material, reduce the hydrophilicity of the filler surface, reduce the swelling effect of gasoline and kerosene on the filler and resin, and the modified filler enhances the interface bonding force between the filler and the epoxy resin, improves the chemical stability of the composite material, and thus reduces the risk of corrosion. At the same time, the impermeability of the bonding material is improved.
[0025] Furthermore, the curing agent is 2,4,6-tris(dimethylaminomethyl)phenol, CAS No.: 90-72-2.
[0026] Furthermore, the defoamer is defoamer BYK088.
[0027] Furthermore, the dispersant is a xylene solution of methyl silicone oil, and the mass concentration of the methyl silicone oil is 1%. The methyl silicone oil is purchased from Jinan Silicon Port Chemical Co., Ltd., model methyl silicone oil 201.
[0028] The present invention also provides a method for preparing a heat-resistant, corrosion-resistant and waterproof epoxy adhesive material, which comprises the following steps: weighing components according to a weight ratio, mixing, stirring for 10-15 minutes at 15-20° C. with a forced mixer, returning to room temperature, and standing for 1-2 hours to obtain a heat-resistant, corrosion-resistant and waterproof epoxy adhesive material.
[0029] The invention also provides application of the heat-resistant, corrosion-resistant and waterproof epoxy bonding material.
[0030] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0031] 1. The temperature difference between day and night will cause the pavement layer and the bridge deck to produce thermal expansion and contraction, and the bonding material is prone to breakage. The present invention compounds three bisphenol A epoxy resins and then modifies them, thereby improving the low temperature resistance of the bonding material. 2. The present invention improves the high temperature resistance of the bonding material by adding a hyperbranched epoxy resin and synergizing with the modified epoxy resin. 3. Gasoline or kerosene leaks may occur during transportation of automobiles, and if not handled in time, it will cause damage to the bridge deck. The present invention can improve the chemical corrosion resistance of the connecting material by adding modified fillers to the bonding material. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] This embodiment provides a heat-resistant, corrosion-resistant and waterproof epoxy adhesive material, comprising the following components in parts by weight: 7 parts of modified epoxy resin, 4 parts of hyperbranched epoxy resin, 5 parts of curing agent, 0.4 parts of dispersant, 0.5 parts of defoaming agent and 9 parts of modified filler;
[0035] The preparation method of the modified epoxy resin is as follows: in a nitrogen environment, 650 parts by mass of bisphenol A epoxy resin is heated to 132° C., 0.6 parts by mass of N,N-dimethylbenzylamine is added, and the reaction is kept warm for 14 hours, and 32 parts by mass of N-methylethanolamine and 206 parts of azobisisobutyronitrile are continuously added, and after reacting at 132° C. for 7 hours, the reaction is cooled to room temperature to obtain the modified epoxy resin.
[0036] The bisphenol A epoxy resin is a mixture of bisphenol A epoxy resin E44, bisphenol A epoxy resin E51 and bisphenol A epoxy resin SP-144 in a mass ratio of 0.3:1.6:1, and was purchased from Jinan Baorui Resin Chemical Co., Ltd.
[0037] The preparation method of the hyperbranched epoxy resin is as follows: under nitrogen protection, 180 parts by mass of glycidyl ether and 9.5 parts by mass of tetrabutylammonium bromide are mixed, heated to 104°C, 11 parts by mass of a trivalent hydroxy compound are added, stirred for 2.5 hours, and 11 parts by mass of the trivalent hydroxy compound are continuously added. After the addition is completed, the mixture is reacted at 104°C for 11 hours. After the reaction is completed, the mixture is cooled to room temperature, 93 parts by mass of tetrahydrofuran is added to dissolve the product, and then the product is precipitated with ethanol for 3 times, and dried at 97°C under vacuum for 12 hours to obtain a hyperbranched epoxy resin.
[0038] The glycidyl ether is a mixture of 1,2-cyclohexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether and propylene glycol triglycidyl ether in a mass ratio of 0.6:1:1.5.
[0039] The trivalent hydroxy compound is a mixture of trimethylolethane, trimethylolpropane and pentaerythritol in a mass ratio of 1:1.3:0.5.
[0040] The preparation method of the modified filler is:
[0041] (1) mixing nano silicon dioxide, nano lanthanum oxide and nano aluminum oxide in a mass ratio of 1:0.5:1.5 to obtain a mixed filler;
[0042] (2) Mixing a mixed filler, a silane coupling agent KH550 and an ethanol aqueous solution with a mass ratio of 1:0.12:12, stirring at 42°C for 1.5 hours, filtering and drying to obtain a silane-modified filler;
[0043] (3) Immerse 1 part by mass of the silane-modified filler in 9 parts by mass of the treatment liquid, treat it ultrasonically for 1.4 hours, filter it out, and then put it into a plasma irradiator for 25 minutes at an irradiation power of 250 W. Then take it out to obtain a modified filler.
[0044] The treatment liquid includes the following components in parts by weight: 13 parts of hexadecyltrimethylammonium bromide, 8 parts of sodium hexametaphosphate, 12 parts of nonylphenol polyoxyethylene ether (NP-10), 9 parts of nano zirconium boride (Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model: ZT-BZr50), and 200 parts of water.
[0045] The average particle size of nano-silicon dioxide is 20nm, and the specific surface area is 180±50m 2 / g.
[0046] The particle size of nano-lanthanum oxide is 30nm-50nm, and the specific surface area is 30-50m 2 / g.
[0047] The average particle size of nano-alumina is 0.3 μm, and the specific surface area is 5-10 m 2 / g.
[0048] The curing agent is 2,4,6-tris(dimethylaminomethyl)phenol, CAS number: 90-72-2.
[0049] The defoaming agent is defoaming agent BYK088.
[0050] The dispersant is a xylene solution of methyl silicone oil, and the mass concentration of the methyl silicone oil is 1%. The methyl silicone oil is purchased from Jinan Silicon Port Chemical Co., Ltd., model methyl silicone oil 201.
[0051] The preparation method of the heat-resistant, corrosion-resistant and waterproof epoxy adhesive material of Example 1 comprises the following steps: weighing the components according to the weight ratio, mixing, stirring at 16° C. for 12 minutes with a forced mixer, returning to room temperature, and standing for 1.6 hours to obtain the heat-resistant, corrosion-resistant and waterproof epoxy adhesive material.
[0052] Example 2
[0053] This embodiment provides a heat-resistant, corrosion-resistant and waterproof epoxy adhesive material, comprising the following components in parts by weight: 5 parts of modified epoxy resin, 3 parts of hyperbranched epoxy resin, 4 parts of curing agent, 0.3 parts of dispersant, 0.2 parts of defoaming agent and 7 parts of modified filler;
[0054] The preparation method of the modified epoxy resin is as follows: in a nitrogen environment, 650 parts by mass of bisphenol A epoxy resin is heated to 130° C., 0.5 parts by mass of N,N-dimethylbenzylamine is added, and the reaction is kept warm for 12 hours, and 30 parts by mass of N-methylethanolamine and 200 parts of azobisisobutyronitrile are continuously added, and after reacting at 130° C. for 6 hours, the reaction is cooled to room temperature to obtain the modified epoxy resin.
[0055] The bisphenol A epoxy resin is a mixture of bisphenol A epoxy resin E44, bisphenol A epoxy resin E51 and bisphenol A epoxy resin SP-144 in a mass ratio of 0.2:1.4:1, and was purchased from Jinan Baorui Resin Chemical Co., Ltd.
[0056] The preparation method of the hyperbranched epoxy resin is as follows: under nitrogen protection, 180 parts by mass of glycidyl ether and 9.2 parts by mass of tetrabutylammonium bromide are mixed, heated to 100°C, 10 parts by mass of a trivalent hydroxy compound are added, stirred for 2 hours, and 10 parts by mass of the trivalent hydroxy compound are continuously added. After the addition is completed, the mixture is reacted at 100°C for 10 hours. After the reaction is completed, the mixture is cooled to room temperature, 90 parts by mass of tetrahydrofuran are added to dissolve the product, and then the product is precipitated with ethanol for 3 times, and dried at 95°C under vacuum for 10 hours to obtain the hyperbranched epoxy resin.
[0057] The glycidyl ether is a mixture of 1,2-cyclohexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether and propylene glycol triglycidyl ether in a mass ratio of 0.5:1:1.3.
[0058] The trivalent hydroxy compound is a mixture of trimethylolethane, trimethylolpropane and pentaerythritol in a mass ratio of 1:1.2:0.4.
[0059] The preparation method of the modified filler is:
[0060] (1) mixing nano silicon dioxide, nano lanthanum oxide and nano aluminum oxide in a mass ratio of 1:0.4:1.3 to obtain a mixed filler;
[0061] (2) Mixing a mixed filler, a silane coupling agent KH550 and a 60% ethanol aqueous solution in a mass ratio of 1:0.1:10, stirring at 40°C for 1 hour, filtering and drying to obtain a silane-modified filler;
[0062] (3) Immerse 1 part by mass of the silane-modified filler in 8 parts by mass of the treatment liquid, treat it ultrasonically for 1 hour, filter it out, and then put it into a plasma irradiator for 20 minutes at an irradiation power of 200 W. Then take it out to obtain a modified filler.
[0063] The treatment liquid includes the following components in parts by weight: 12 parts of hexadecyltrimethylammonium bromide, 6 parts of sodium hexametaphosphate, 10 parts of nonylphenol polyoxyethylene ether (NP-10), 7 parts of nano-zirconium boride (Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model: ZT-BZr50), and 200 parts of water.
[0064] The average particle size of nano-silicon dioxide is 20nm, and the specific surface area is 180±50m 2 / g.
[0065] The particle size of nano-lanthanum oxide is 30nm-50nm, and the specific surface area is 30-50m 2 / g.
[0066] The average particle size of nano-alumina is 0.3 μm, and the specific surface area is 5-10 m 2 / g.
[0067] The curing agent is 2,4,6-tris(dimethylaminomethyl)phenol, CAS number: 90-72-2.
[0068] The defoaming agent is defoaming agent BYK088.
[0069] The dispersant is a xylene solution of methyl silicone oil, and the mass concentration of the methyl silicone oil is 1%. The methyl silicone oil is purchased from Jinan Silicon Port Chemical Co., Ltd., model methyl silicone oil 201.
[0070] The preparation method of the heat-resistant, corrosion-resistant and waterproof epoxy adhesive material of Example 2 comprises the following steps: weighing the components according to the weight ratio, mixing, stirring for 10 minutes at 15°C with a forced mixer, returning to room temperature, and standing for 1 hour to obtain the heat-resistant, corrosion-resistant and waterproof epoxy adhesive material.
[0071] Example 3
[0072] This embodiment provides a heat-resistant, corrosion-resistant and waterproof epoxy adhesive material, comprising the following components in parts by weight: 9 parts of a modified epoxy resin, 6 parts of a hyperbranched epoxy resin, 6 parts of a curing agent, 0.5 parts of a dispersant, 0.6 parts of a defoaming agent and 10 parts of a modified filler;
[0073] The preparation method of the modified epoxy resin is as follows: in a nitrogen environment, 650 parts by mass of bisphenol A epoxy resin is heated to 135° C., 0.7 parts by mass of N,N-dimethylbenzylamine is added, and the mixture is kept warm for reaction for 15 hours, 35 parts by mass of N-methylethanolamine and 210 parts of azobisisobutyronitrile are continuously added, and the mixture is reacted at 135° C. for 8 hours, and then cooled to room temperature to obtain the modified epoxy resin.
[0074] The bisphenol A epoxy resin is a mixture of bisphenol A epoxy resin E44, bisphenol A epoxy resin E51 and bisphenol A epoxy resin SP-144 in a mass ratio of 0.5:1.7:1, and was purchased from Jinan Baorui Resin Chemical Co., Ltd.
[0075] The preparation method of the hyperbranched epoxy resin is as follows: under nitrogen protection, 180 parts by mass of glycidyl ether and 9.7 parts by mass of tetrabutylammonium bromide are mixed, heated to 110°C, 12 parts by mass of a trivalent hydroxy compound are added, stirred for 3 hours, and 12 parts by mass of the trivalent hydroxy compound are continuously added. After the addition is completed, the mixture is reacted at 110°C for 12 hours. After the reaction is completed, the mixture is cooled to room temperature, 95 parts by mass of tetrahydrofuran are added to dissolve the product, and then the product is precipitated with ethanol for 4 times, and dried at 100°C in a vacuum state for 15 hours to obtain the hyperbranched epoxy resin.
[0076] The glycidyl ether is a mixture of 1,2-cyclohexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether and glycerol triglycidyl ether in a mass ratio of 0.8:1:1.6.
[0077] The trivalent hydroxy compound is a mixture of trimethylolethane, trimethylolpropane and pentaerythritol in a mass ratio of 1:1.5:0.7.
[0078] The preparation method of the modified filler is:
[0079] (1) mixing nano silicon dioxide, nano lanthanum oxide and nano aluminum oxide in a mass ratio of 1:0.6:1.6 to obtain a mixed filler;
[0080] (2) Mixing a mixed filler, a silane coupling agent KH550 and an ethanol aqueous solution with a mass ratio of 1:0.15:15, stirring at 45°C for 2 hours, filtering and drying to obtain a silane-modified filler;
[0081] (3) Immerse 1 part by mass of the silane-modified filler in 10 parts by mass of the treatment liquid, treat it ultrasonically for 2 hours, filter it out, and then put it into a plasma irradiator for 30 minutes at an irradiation power of 300 W. Then take it out to obtain a modified filler.
[0082] The treatment liquid includes the following components in parts by weight: 14 parts of hexadecyltrimethylammonium bromide, 9 parts of sodium hexametaphosphate, 13 parts of nonylphenol polyoxyethylene ether (NP-10), 10 parts of nano zirconium boride (Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model: ZT-BZr50), and 200 parts of water.
[0083] The average particle size of nano-silicon dioxide is 20nm, and the specific surface area is 180±50m 2 / g.
[0084] The particle size of nano-lanthanum oxide is 30nm-50nm, and the specific surface area is 30-50m 2 / g.
[0085] The average particle size of nano-alumina is 0.3 μm, and the specific surface area is 5-10 m 2 / g.
[0086] The curing agent is 2,4,6-tris(dimethylaminomethyl)phenol, CAS number: 90-72-2.
[0087] The defoaming agent is defoaming agent BYK088.
[0088] The dispersant is a xylene solution of methyl silicone oil, and the mass concentration of the methyl silicone oil is 1%. The methyl silicone oil is purchased from Jinan Silicon Port Chemical Co., Ltd., model methyl silicone oil 201.
[0089] The preparation method of the heat-resistant, corrosion-resistant and waterproof epoxy adhesive material of Example 3 comprises the following steps: weighing the components according to the weight ratio, mixing, stirring for 15 minutes at 20°C with a forced mixer, returning to room temperature, and standing for 2 hours to obtain the heat-resistant, corrosion-resistant and waterproof epoxy adhesive material.
[0090] Comparative Example 1
[0091] The difference between this comparative example and Example 1 is: 3 parts of modified epoxy resin and 8 parts of hyperbranched epoxy resin.
[0092] Comparative Example 2
[0093] The difference between this comparative example and Example 1 is that the bisphenol A epoxy resin is a mixture of bisphenol A epoxy resin E44, bisphenol A epoxy resin E51 and bisphenol A epoxy resin SP-144 in a mass ratio of 1:1:1.
[0094] Comparative Example 3
[0095] The difference between this comparative example and Example 1 is that the glycidyl ether is a mixture of 1,2-cyclohexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether and propylene glycol triglycidyl ether in a mass ratio of 1:1:1.
[0096] Comparative Example 4
[0097] The difference between this comparative example and Example 1 is that the trivalent hydroxy compound is a mixture of trimethylolethane, trimethylolpropane and pentaerythritol in a mass ratio of 1:1:1.
[0098] Comparative Example 5
[0099] The difference between this comparative example and Example 1 is that nano silicon dioxide, nano lanthanum oxide and nano aluminum oxide are mixed in a mass ratio of 1:1:1 to obtain a mixed filler.
[0100] Comparative Example 6
[0101] The difference between this comparative example and Example 1 is that the average particle size of the nano-silicon dioxide is 80 nm, and the specific surface area is 60 ± 20 m 2 / g. The particle size of nano-lanthanum oxide is 1μm-5μm, and the specific surface area is 1-10m 2 / g. The average particle size of nano-alumina is 10μm, and the specific surface area is 1-5m 2 / g.
[0102] Comparative Example 7
[0103] The difference between this comparative example and Example 1 is that nano silicon dioxide is replaced by boron carbide (Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model: ZT-BC60); nano lanthanum oxide is replaced by titanium dioxide (Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model: ZT05N); nano aluminum oxide is replaced by zinc oxide (Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model: ZT-AZO)
[0104] Performance Testing
[0105] The products prepared in Examples 1-3 and Comparative Examples 1-7 were subjected to performance tests.
[0106] 1. Refer to JTT712-2008, keep at -10℃ for 4h and place at room temperature for 4h as one cycle. After three consecutive cycles, measure the low-temperature crack resistance.
[0107] 2. Refer to JTT712-2008, keep at 50℃ for 4h and place at room temperature for 4h as one cycle. After three consecutive cycles, measure the high temperature crack resistance.
[0108] 3. Refer to JTT712-2008, immerse in gasoline and kerosene for 24 hours respectively, and measure the corrosion resistance.
[0109] 4. Refer to GB / T16777-2008, 0.3MPa, 120min, to measure the impermeability.
[0110] 5. Refer to GB / T16777-2008, and measure the tensile strength and elongation at break at 23℃.
[0111] The results are shown in Table 1.
[0112] Table 1 Performance test results
[0113]
[0114] It can be seen from the above performance test results that the comprehensive performance of Examples 1-3 is excellent, especially the comprehensive performance of Example 1 is the most outstanding, which is mainly due to the synergistic effect of multiple components.
[0115] However, the comparative examples are obviously inferior to the embodiments in the corresponding performance tests because they do not adopt the necessary technical solutions. In comparative example 1, the ratio of the modified epoxy resin and the hyperbranched epoxy resin is changed, and it can be seen that the comprehensive effect decreases, proving that the two epoxy resin ratio schemes have an important influence on the comprehensive effect. The mass ratios of the various components in the bisphenol A epoxy resin in comparative example 2 are different, and it can be seen from the results that the low temperature resistance effect is affected. The different distribution ratios of the various groups in the reaction raw materials for preparing the hyperbranched epoxy resin in comparative examples 3-4 can be seen from the results that the high temperature resistance effect is affected. The different distribution ratios of the various groups in the fillers used in the preparation of the modified fillers in comparative example 5, and the parameters and types of the fillers are changed in comparative examples 6-7, which affect the corrosion resistance and water resistance. The above experimental results further prove the importance of the technical solution defined in the present invention for its technical effects.
[0116] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A heat-resistant, corrosion-resistant and waterproof epoxy bonding material, characterized in that: The invention comprises the following components in parts by weight: 5-9 parts of modified epoxy resin, 3-6 parts of hyperbranched epoxy resin, 4-6 parts of curing agent, 0.3-0.5 parts of dispersant, 0.2-0.6 parts of defoaming agent and 7-10 parts of modified filler; The preparation method of the modified epoxy resin is as follows: in a nitrogen environment, 650 parts by weight of bisphenol A epoxy resin is heated to 130-135° C., 0.5-0.7 parts by weight of N,N-dimethylbenzylamine is added, the reaction is carried out by heat preservation for 12-15 hours, 30-35 parts by weight of N-methylethanolamine and 200-210 parts of azobisisobutyronitrile are continuously added, the reaction is carried out at 130-135° C. for 6-8 hours, and the reaction is cooled to room temperature to obtain the modified epoxy resin; The bisphenol A epoxy resin is a mixture of bisphenol A epoxy resin E44, bisphenol A epoxy resin E51 and bisphenol A epoxy resin SP-144 in a mass ratio of (0.2-0.5):(1.4-1.7):1; The preparation method of the hyperbranched epoxy resin is as follows: under nitrogen protection, 180 parts by weight of glycidyl ether and 9.2-9.7 parts by weight of tetrabutylammonium bromide are mixed, heated to 100-110° C., 10-12 parts by weight of a trivalent hydroxy compound are added, stirred for 2-3 hours, and 10-12 parts by weight of the trivalent hydroxy compound are continuously added. After the addition is completed, the mixture is reacted at 100-110° C. for 10-12 hours. After the reaction is completed, the mixture is cooled to room temperature, 90-95 parts by weight of tetrahydrofuran are added to dissolve the product, and then the product is precipitated with ethanol for 3-4 times, and dried at 95-100° C. under vacuum for 10-15 hours to obtain the hyperbranched epoxy resin; The glycidyl ether is a mixture of 1,2-cyclohexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether and propylene glycol triglycidyl ether in a mass ratio of (0.5-0.8):1:(1.3-1.6); The trivalent hydroxy compound is a mixture of trimethylolethane, trimethylolpropane and pentaerythritol in a mass ratio of 1: (1.2-1.5): (0.4-0.7); The preparation method of the modified filler is: (1) Mixing nano silicon dioxide, nano lanthanum oxide and nano aluminum oxide in a mass ratio of 1: (0.4-0.6): (1.3-1.6) to obtain a mixed filler; (2) Mixing a mixed filler in a mass ratio of 1: (0.1-0.15): (10-15), a silane coupling agent KH550 and an ethanol aqueous solution with a mass fraction of 60-70%, stirring at 40-45° C. for 1-2 hours, filtering, and drying to obtain a silane-modified filler; (3) immersing 1 part by mass of the silane-modified filler into 8-10 parts by mass of the treatment liquid, subjecting it to ultrasonic treatment for 1-2 hours, filtering it out, and then placing it in a plasma radiation instrument, subjecting it to plasma radiation treatment at an irradiation power of 200-300 W for 20-30 minutes, and taking it out to obtain a modified filler; The treatment liquid comprises the following components in parts by weight: 12-14 parts of hexadecyltrimethylammonium bromide, 6-9 parts of sodium hexametaphosphate, 10-13 parts of nonylphenol polyoxyethylene ether, 7-10 parts of nano zirconium boride and 200 parts of water; The average particle size of nano-silicon dioxide is 20nm, and the specific surface area is 180±50m 2 / g; the particle size of nano lanthanum oxide is 30nm-50nm, and the specific surface area is 30-50m 2 / g; the average particle size of nano-alumina is 0.3μm, and the specific surface area is 5-10m 2 / g.
2. A method for preparing the heat-resistant, corrosion-resistant and waterproof epoxy adhesive material according to claim 1, characterized in that: The method comprises the following steps: weighing components according to weight ratio, mixing, stirring for 10-15 minutes at 15-20° C. with a forced mixer, returning to room temperature, and standing for 1-2 hours to obtain a heat-resistant, corrosion-resistant and waterproof epoxy bonding material.
3. Use of the heat-resistant, corrosion-resistant and waterproof epoxy adhesive material according to claim 1 in road materials.
Citation Information
Patent Citations
High-precision alumina polishing solution and preparation method thereof
CN101831244A
Flame-retardant heating structure bonding polymer adhesive
CN116875251A
Two-component flexible epoxy glue and preparation method thereof
CN117343683A
Economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility as well as preparation method thereof
US20230407083A1
Epoxy resin, process for the preparation thereof and process for the production of epoxy foam
US5166184A