Nitrile rubber chemical foaming material and preparation method thereof

By modifying nitrile rubber, epoxy groups and bromine-tetraethylene glycol-carboxylic acid are introduced, and polyether segments are introduced on the fluoroelastomer, the nitrile rubber is solved to harden and brittle at low temperatures. The problem of this material has achieved good oil resistance and low temperature resistance, and is suitable for industrial production.

CN118909334AInactive Publication Date: 2024-11-08CHANGZHOU QIANFENG PLASTIC PROD FACTORY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411166907.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Nitrile rubber has problems such as hardening and brittleness and loss of mechanical properties at low temperatures, which leads to a contradiction between its oil resistance and low temperature resistance. The existing nitrile rubber foaming materials are inconvenient to operate in industrial production, and the addition of plasticizers is affected. The size and uniformity of the cell affect the quality of the material.

Method used

By modifying nitrile rubber, epoxy groups and bromine-tetrapolymer glycol-carboxylic acid are introduced to increase in molecular force and flexibility, and polyether segments are introduced on fluoroelastomer to improve its oil resistance and low temperature resistance, while optimizing formulation and process, including specific ratio vulcanizing agents and foaming agents to ensure the foam density and compatibility of the material.

Benefits of technology

It has achieved good foaming density, oil resistance and low temperature resistance of nitrile rubber chemical foaming materials, improved processing performance, and improved the overall performance of the material, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of rubber foaming materials, in particular to a nitrile rubber chemical foaming material which comprises the following raw materials in parts by weight: 40-50 parts of modified nitrile rubber, 1-3 parts of a vulcanizing agent, 1-5 parts of a vulcanization accelerator, 1-3 parts of an activating agent, 1-3 parts of a foaming agent, 10-20 parts of calcium carbonate and 2-4 parts of an anti-aging agent. The nitrile rubber chemical foaming material prepared by the invention has good oil resistance and low temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of rubber foaming materials, and in particular to a nitrile rubber chemical foaming material and a preparation method thereof. Background Art

[0002] The molecular chain structure of nitrile rubber is highly saturated and contains a strong polar group cyanide. It is a rubber elastomer that combines oil resistance, aging resistance, heat resistance, chemical resistance and excellent mechanical properties. It is widely used in the fields of automobiles, aerospace, petrochemicals, pharmaceuticals, sealing products, etc. In order to better meet the use requirements in harsh environments, in recent years, scientific researchers have been committed to the modification of nitrile rubber and the development of rubber materials that can be used under extreme conditions. Due to the characteristics of the molecular structure of nitrile rubber, oil resistance will increase with the increase of cyanide content, but at the same time it will lead to an increase in the glass transition temperature, making nitrile rubber hard and brittle at low temperatures, and seriously losing mechanical properties. Therefore, the contradiction between oil resistance and low temperature resistance of nitrile rubber limits its application.

[0003] Compared with nitrile rubber, nitrile rubber foam material has the advantages of light weight, high strength and low cost, and is gradually favored by the fields of building materials, automobiles and ships, aerospace, medical equipment, etc. However, most nitrile rubbers on the market need to add plasticizers to improve the processing performance of nitrile rubber. However, the addition of plasticizers will affect the size and uniformity of the bubbles and affect the quality of the foam material.

[0004] Patent CN107200879B discloses a nitrile rubber microporous foam material and a preparation method thereof, wherein the formula includes a nitrile rubber blend, a stabilizer, a filler, a plasticizer, a vulcanizer, a vulcanization accelerator, an active agent and an antioxidant, and carbon dioxide and nitrogen are introduced as physical foaming agents to prepare a foam material having the advantage of a small pore diameter. However, this method is difficult to operate and is not suitable for industrial production.

[0005] Patent CN109880196B discloses a nitrile rubber composition and its foaming material, the formula of which includes nitrile rubber, phenolic resin, polyvinyl butyral and a modifier. The phenolic resin is used as a vulcanizing agent to solve the problem of corrosion of metal pipes caused by the conventional use of sulfur as a vulcanizing agent. However, the cost of phenolic resin as a vulcanizing agent is relatively high and it will affect the oil resistance of the nitrile rubber itself.

[0006] Therefore, there is an urgent need in the market for a nitrile rubber chemical foaming material with good oil resistance and low temperature resistance. Summary of the invention

[0007] In view of the problems existing in the prior art, the object of the present invention is to obtain a nitrile rubber chemical foaming material with good oil resistance and low temperature resistance.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] On one hand, the present invention provides a nitrile rubber chemical foaming material, which comprises the following raw materials, measured in parts by weight: 40-50 parts of modified nitrile rubber, 1-3 parts of a vulcanizing agent, 1-5 parts of a vulcanization accelerator, 1-3 parts of an activator, 1-3 parts of a foaming agent, 10-20 parts of calcium carbonate, and 2-4 parts of an antioxidant.

[0010] The present invention discloses a nitrile rubber chemical foaming material prepared by modifying nitrile rubber and mixing the nitrile rubber with an auxiliary agent and a foaming agent, which has good foaming density, oil resistance and low temperature resistance.

[0011] In some embodiments, the method for preparing the modified nitrile rubber comprises the following steps:

[0012] A1, adding nitrile rubber and chlorobenzene to a reaction vessel, stirring at room temperature until the nitrile rubber is dissolved, adding acetic acid and 66-70wt% aqueous hydrogen peroxide solution, heating to 55-65°C for reaction for 5-7h, cooling to room temperature, adding ethanol and stirring for 20-30min, taking out the precipitate, and drying to obtain epoxidized nitrile rubber;

[0013] A2. Add the epoxidized nitrile rubber and chlorobenzene obtained in step A1 into a reaction vessel, stir at room temperature until the epoxidized nitrile rubber is dissolved, then add brominated-tetraethylene glycol-carboxylic acid and ferric bromide, heat to 120-140 ° C and react for 3-5 hours, cool to room temperature, add ethanol and stir for 20-30 minutes, take out the precipitate, and obtain modified nitrile rubber after drying.

[0014] The present application introduces epoxy groups into the nitrile rubber, and after epoxidation, the polarity of the rubber macromolecule increases, the intermolecular force is enhanced, and it is difficult for gas and non-polar oil agents to penetrate into the nitrile rubber molecular chain segment, thereby improving the oil resistance of the nitrile rubber foam material. In addition, the present application makes some epoxy groups react with bromo-tetraethylene glycol-carboxylic acid grafting. On the one hand, bromine atoms are introduced into the nitrile rubber chain segment, which can promote the vulcanization of the nitrile rubber chain segment to improve its oil resistance; on the other hand, the introduction of polyethylene glycol chain segment improves the flexibility of the nitrile rubber chain segment, ensuring that the nitrile rubber has both oil resistance and low temperature resistance. At the same time, the polyethylene glycol chain segment can play the role of a plasticizer, promote the compatibility of the filler and the resin body, and improve the processing performance of the nitrile rubber.

[0015] In some embodiments, the weight ratio of the nitrile rubber, acetic acid and 66-70 wt % aqueous hydrogen peroxide solution in step A1 is 1:(0.15-0.2):(0.8-1).

[0016] The present application selects a specific ratio of acetic acid and a 66-70wt% aqueous hydrogen peroxide solution to form peracetic acid to react with nitrile rubber, so that the nitrile rubber chemical foaming material can have good oil resistance. This may be because the introduction of epoxy groups may affect the number of double bonds in the nitrile rubber, thereby affecting the vulcanization effect of the nitrile rubber.

[0017] In some embodiments, the weight ratio of the epoxidized nitrile rubber to the brominated-tetraethylene glycol-carboxylic acid in step A2 is 1:(0.05-0.1).

[0018] The present application selects a specific ratio of brominated-tetraethylene glycol-carboxylic acid as a modifier for epoxidized nitrile rubber, so that the nitrile rubber has better oil resistance. This may be because brominated-tetraethylene glycol-carboxylic acid, when the acidity in the rubber system is too high, will corrode the nitrile rubber and break the molecular chains between the rubbers, thereby reducing the oil resistance of the nitrile rubber chemical foaming material.

[0019] In some embodiments, the vulcanizing agent is a combination of S-80 and zinc oxide, and the weight ratio of the two is 1:(1-2).

[0020] The present invention does not impose any particular limitation on the vulcanization accelerator, which can be purchased commercially.

[0021] Preferably, the vulcanization accelerator is CZ.

[0022] The present invention does not impose any special restrictions on the antioxidant, which can be purchased commercially.

[0023] Preferably, the antioxidant is antioxidant KY-405.

[0024] The present invention does not impose any special limitation on the activator, and the activator can be purchased commercially.

[0025] Preferably, the activator is stearic acid.

[0026] In some embodiments, the foaming agent is diisopropyl azodicarboxylate and sodium bicarbonate, and the weight ratio of the two is 1:(0.4-0.6).

[0027] In some embodiments, the nitrile rubber chemical foaming material further contains 10-20 parts by weight of modified fluororubber.

[0028] In some embodiments, the method for preparing the modified fluororubber comprises the following steps:

[0029] B1. Add acrylic acid, fluororubber and benzoyl peroxide into a reaction vessel, and react at 70-80° C. for 2-4 hours to obtain acrylic acid-modified fluororubber;

[0030] B2. Add the acrylic modified fluororubber, polyether and phosphoric acid obtained in step B1 into a reaction vessel, heat to 70-80° C. and react for 2-4 hours to obtain modified fluororubber.

[0031] In some embodiments, the polyether is one or more of polypropylene glycol, polyethylene glycol, and polytetrahydrofuran.

[0032] Preferably, the polyether is polypropylene glycol.

[0033] The present application further adds fluororubber to nitrile rubber. Fluororubber has good low temperature resistance and oil resistance. Blending with nitrile rubber can further increase the various properties of nitrile rubber. However, the compatibility of fluororubber and nitrile rubber system is poor. The present application introduces polyether segments into fluororubber to improve the compatibility of fluororubber and nitrile rubber on the one hand, and further improve the low temperature resistance of fluororubber on the other hand. In addition, the polyether segments can act as a foam stabilizer during the foaming process of rubber, making the foaming of each part of the rubber more uniform.

[0034] In some embodiments, the weight ratio of acrylic acid to fluororubber in step B1 is (0.04-0.06):1.

[0035] The present application can make the nitrile rubber chemical foaming material have better foaming performance by selecting a specific ratio of acrylic acid and fluororubber to react. This may be because the residual carboxyl group in the system can play the role of a co-foaming agent for the organic foaming agent.

[0036] In some embodiments, the weight ratio of acrylic modified fluororubber to polyether in step B2 is 1:(0.1-0.3).

[0037] The present application can make the nitrile rubber chemical foaming material have better foaming performance by selecting a specific ratio of acrylic modified fluororubber and polyether, which may be because the residual polyether can stabilize the structure of the pores.

[0038] Another aspect of the present invention provides a method for preparing a chemical foamed nitrile rubber material, comprising the following steps:

[0039] (1) placing the modified nitrile rubber in an open mill for plasticizing at a temperature of 70-80° C. for a plasticizing time of 1-2 h to obtain a plasticized rubber;

[0040] (2) pouring the plasticized rubber, vulcanizing agent, vulcanization accelerator, calcium carbonate, foaming agent and antioxidant obtained in step (1) into an open mill and rolling them together until the rubber material is coated with rollers without viscous liquid on the surface, and then leaving the rolls for 2 to 3 days to form, thereby obtaining a formed rubber;

[0041] (3) vulcanizing and foaming the molded rubber obtained in step (2) in a flat vulcanizer to obtain the nitrile rubber chemical foaming material, wherein the vulcanization temperature is 165-170° C. and the vulcanization time is 10-20 min.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] (1) The present invention modifies nitrile rubber and mixes it with an auxiliary agent and a foaming agent to prepare a nitrile rubber chemical foaming material having good foaming density, oil resistance and low temperature resistance.

[0044] (2) The present invention introduces epoxy groups into nitrile rubber and reacts some of the epoxy groups with brominated-tetraethylene glycol-carboxylic acid, thereby introducing bromine atoms and polyethylene glycol segments into the nitrile rubber chain segments, thereby improving the flexibility, oil resistance and low temperature resistance of the nitrile rubber chain segments, and can also enhance the processing performance of the nitrile rubber chemical foaming material.

[0045] (3) The present invention further improves the low temperature resistance and oil resistance of the nitrile rubber chemical foaming material by introducing fluororubber into nitrile rubber, and introduces polyether segments into the fluororubber to improve the compatibility between fluororubber and nitrile rubber on the one hand, and further improve the low temperature resistance of the fluororubber on the other hand. In addition, the residual carboxyl groups in the system can play the role of a co-foaming agent for the organic foaming agent, and the residual polyether can stabilize the structure of the pores. DETAILED DESCRIPTION

[0046] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0047] In the following embodiments and comparative examples, except for modified nitrile rubber and modified fluororubber, the other compounds and related reagents used can be purchased from the market, among which, the model of nitrile rubber is 1945GRN, purchased from Guangzhou Degao New Materials Co., Ltd.; the model of fluororubber is FE2603, purchased from Dongguan Weicai Plastic Raw Materials Co., Ltd.; the number average molecular weight of polypropylene glycol is 1000, purchased from Dongguan Weicai Plastic Raw Materials Co., Ltd.; brominated-tetraethylene glycol-carboxylic acid is purchased from Shaanxi Xinyan Bomei Biotechnology Co., Ltd.; S-80 and CZ are both purchased from Guangzhou Lida Rubber Raw Materials Trading Co., Ltd.

[0048] Preparation Example 1

[0049] The preparation method of modified nitrile rubber-1 comprises the following steps:

[0050] A1, 10g of nitrile rubber and 100g of chlorobenzene were added to a reaction vessel, stirred at room temperature until the nitrile rubber was dissolved, 1.7g of acetic acid and 9g of 68wt% aqueous hydrogen peroxide solution were added, the temperature was raised to 60°C for reaction for 6h, cooled to room temperature, added to 20g of anhydrous ethanol and stirred for 25min, the precipitate was taken out, and the epoxidized nitrile rubber was obtained after drying;

[0051] A2. Add 10 g of the epoxidized nitrile rubber obtained in step A1 and 100 g of chlorobenzene into a reaction vessel, stir at room temperature until the epoxidized nitrile rubber is dissolved, then add 0.7 g of bromo-tetraethylene glycol-carboxylic acid and 0.1 g of ferric bromide, heat to 130 ° C and react for 4 h, cool to room temperature, add 20 g of anhydrous ethanol and stir for 25 min, take out the precipitate, and obtain modified nitrile rubber-1 after drying.

[0052] Preparation Example 2

[0053] The preparation method of modified nitrile rubber-2 comprises the following steps:

[0054] A1, 10g of nitrile rubber and 100g of chlorobenzene were added to a reaction vessel, stirred at room temperature until the nitrile rubber was dissolved, 2.5g of acetic acid and 9g of 68wt% aqueous hydrogen peroxide solution were added, the temperature was raised to 60°C for reaction for 6h, cooled to room temperature, added to 20g of anhydrous ethanol and stirred for 25min, the precipitate was taken out, and the epoxidized nitrile rubber was obtained after drying;

[0055] A2. Add 10 g of the epoxidized nitrile rubber obtained in step A1 and 100 g of chlorobenzene into a reaction vessel, stir at room temperature until the epoxidized nitrile rubber is dissolved, then add 0.7 g of bromo-tetraethylene glycol-carboxylic acid and 0.1 g of ferric bromide, heat to 130 ° C and react for 4 h, cool to room temperature, add 20 g of anhydrous ethanol and stir for 25 min, take out the precipitate, and obtain modified nitrile rubber-2 after drying.

[0056] Preparation Example 3

[0057] The preparation method of modified nitrile rubber-3 comprises the following steps:

[0058] A1, 10g of nitrile rubber and 100g of chlorobenzene were added to a reaction vessel, stirred at room temperature until the nitrile rubber was dissolved, 2.5g of acetic acid and 9g of 68wt% aqueous hydrogen peroxide solution were added, the temperature was raised to 60°C for reaction for 6h, cooled to room temperature, added to 20g of anhydrous ethanol and stirred for 25min, the precipitate was taken out, and the epoxidized nitrile rubber was obtained after drying;

[0059] A2. Add 10 g of the epoxidized nitrile rubber obtained in step A1 and 100 g of chlorobenzene into a reaction vessel, stir at room temperature until the epoxidized nitrile rubber is dissolved, then add 1.2 g of bromo-tetraethylene glycol-carboxylic acid and 0.1 g of ferric bromide, heat to 130 ° C and react for 4 h, cool to room temperature, add 20 g of anhydrous ethanol and stir for 25 min, take out the precipitate, and obtain modified nitrile rubber-3 after drying.

[0060] Preparation Example 4

[0061] The preparation method of the vulcanizing agent is as follows: 10 g of S-80 and 15 g of zinc oxide are added into a container, and stirred at room temperature for 20 minutes to obtain the vulcanizing agent.

[0062] Preparation Example 5

[0063] The preparation method of the foaming agent is as follows: 10 g of diisopropyl azodicarboxylate and 5 g of sodium bicarbonate are added into a container, and stirred at room temperature for 20 minutes to obtain the foaming agent.

[0064] Preparation Example 6

[0065] The preparation method of modified fluororubber-1 comprises the following steps:

[0066] B1, adding 0.5g acrylic acid, 10g fluororubber and 0.1g benzoyl peroxide into a reaction container, reacting at 75°C for 3h to obtain acrylic acid modified fluororubber;

[0067] B2. Add 10 g of the acrylic modified fluororubber obtained in step B1, 2 g of polypropylene glycol and 0.1 g of 85 wt % phosphoric acid into a reaction container, heat to 75° C. and react for 3 h to obtain modified fluororubber-1.

[0068] Preparation Example 7

[0069] The preparation method of modified fluororubber-2 comprises the following steps:

[0070] B1, 0.3 g acrylic acid, 10 g fluororubber and 0.1 g benzoyl peroxide were added into a reaction vessel, and reacted at 75° C. for 3 h to obtain acrylic acid modified fluororubber;

[0071] B2. Add 10 g of the acrylic modified fluororubber obtained in step B1, 2 g of polypropylene glycol and 0.1 g of 85 wt % phosphoric acid into a reaction container, heat to 75° C. and react for 3 h to obtain modified fluororubber-2.

[0072] Preparation Example 8

[0073] The preparation method of modified fluororubber-3 comprises the following steps:

[0074] B1, adding 0.5g acrylic acid, 10g fluororubber and 0.1g benzoyl peroxide into a reaction container, reacting at 75°C for 3h to obtain acrylic acid modified fluororubber;

[0075] B2. Add 10 g of the acrylic modified fluororubber obtained in step B1, 0.5 g of polypropylene glycol and 0.1 g of 85 wt % phosphoric acid into a reaction container, heat to 75° C. and react for 3 h to obtain modified fluororubber-3.

[0076] Example 1

[0077] A nitrile rubber chemical foaming material comprises the following raw materials, measured by weight: 145 parts of modified nitrile rubber, 2 parts of vulcanizing agent, 3 parts of CZ, 2 parts of stearic acid, 2 parts of foaming agent, 15 parts of calcium carbonate and 3 parts of antioxidant KY-405.

[0078] The preparation method of the nitrile rubber chemical foaming material of this embodiment comprises the following steps:

[0079] (1) placing modified nitrile rubber-1 into an open mill for plasticizing at a temperature of 75° C. for a plasticizing time of 1.5 h to obtain a plasticized rubber;

[0080] (2) pouring the plasticized rubber obtained in step (1), the vulcanizing agent, CZ, stearic acid, the foaming agent, calcium carbonate, and the antioxidant KY-405 into an open mill at the same time and rolling them together until the rubber material is coated with the roller without viscous liquid on the surface, and then leaving the sheet to stand for 2 days to form a formed rubber;

[0081] (3) vulcanizing and foaming the molded rubber obtained in step (2) in a flat vulcanizer to obtain the nitrile rubber chemical foaming material, wherein the vulcanization temperature is 168° C. and the vulcanization time is 15 min.

[0082] Example 2

[0083] A nitrile rubber chemical foaming material comprises the following raw materials, measured by weight: 140 parts of modified nitrile rubber, 1 part of vulcanizing agent, 1 part of CZ, 1 part of stearic acid, 1 part of foaming agent, 10 parts of calcium carbonate and 2 parts of antioxidant KY-405.

[0084] The preparation method of the nitrile rubber chemical foaming material of this embodiment comprises the following steps:

[0085] (1) placing modified nitrile rubber-1 into an open mill for plasticizing at a temperature of 70° C. for 1 h to obtain a plasticized rubber;

[0086] (2) pouring the plasticized rubber obtained in step (1), the vulcanizing agent, CZ, stearic acid, the foaming agent, calcium carbonate, and the antioxidant KY-405 into an open mill at the same time and rolling them together until the rubber material is coated with the roller without viscous liquid on the surface, and then leaving the sheet to stand for 2 days to form a formed rubber;

[0087] (3) vulcanizing and foaming the molded rubber obtained in step (2) in a flat vulcanizer to obtain the nitrile rubber chemical foaming material, wherein the vulcanization temperature is 165° C. and the vulcanization time is 20 min.

[0088] Example 3

[0089] A nitrile rubber chemical foaming material comprises the following raw materials, measured by weight: 150 parts of modified nitrile rubber, 3 parts of vulcanizing agent, 5 parts of CZ, 3 parts of stearic acid, 3 parts of foaming agent, 20 parts of calcium carbonate and 4 parts of antioxidant KY-405.

[0090] The preparation method of the nitrile rubber chemical foaming material of this embodiment comprises the following steps:

[0091] (1) placing modified nitrile rubber-1 into an open mill for plasticizing at a temperature of 80° C. for a plasticizing time of 2 h to obtain a plasticized rubber;

[0092] (2) pouring the plasticized rubber obtained in step (1), the vulcanizing agent, CZ, stearic acid, the foaming agent, calcium carbonate, and the antioxidant KY-405 into an open mill at the same time and rolling them together until the rubber material is coated with the roller without viscous liquid on the surface, and then leaving the sheet to stand for 3 days to form a formed rubber;

[0093] (3) vulcanizing and foaming the molded rubber obtained in step (2) in a flat vulcanizer to obtain the nitrile rubber chemical foaming material, wherein the vulcanization temperature is 170° C. and the vulcanization time is 10 min.

[0094] Example 4

[0095] A nitrile rubber chemical foaming material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified nitrile rubber-1 is replaced by modified nitrile rubber-2.

[0096] Example 5

[0097] A nitrile rubber chemical foaming material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified nitrile rubber-1 is replaced by modified nitrile rubber-3.

[0098] Example 6

[0099] A nitrile rubber chemical foaming material comprises the following raw materials, measured by weight: 140 parts of modified nitrile rubber, 1 part of vulcanizing agent, 1 part of CZ, 1 part of stearic acid, 1 part of foaming agent, 10 parts of calcium carbonate, 2 parts of antioxidant KY-405, and 115 parts of modified fluororubber.

[0100] The preparation method of the nitrile rubber chemical foaming material of this embodiment comprises the following steps:

[0101] (1) placing modified nitrile rubber-1 and modified fluororubber-1 in an open mill for plasticizing at a plasticizing temperature of 70° C. for a plasticizing time of 1 h to obtain plasticized rubber;

[0102] (2) pouring the plasticized rubber obtained in step (1), the vulcanizing agent, CZ, stearic acid, the foaming agent, calcium carbonate, and the antioxidant KY-405 into an open mill at the same time and rolling them together until the rubber material is coated with the roller without viscous liquid on the surface, and then leaving the sheet to stand for 2 days to form a formed rubber;

[0103] (3) vulcanizing and foaming the molded rubber obtained in step (2) in a flat vulcanizer to obtain the nitrile rubber chemical foaming material, wherein the vulcanization temperature is 165° C. and the vulcanization time is 10 min.

[0104] Example 7

[0105] A nitrile rubber chemical foaming material and a preparation method thereof. The specific implementation method is the same as Example 6, except that the modified fluororubber-1 is replaced by modified fluororubber-2 in equal amounts.

[0106] Example 8

[0107] A nitrile rubber chemical foaming material and a preparation method thereof. The specific implementation method is the same as Example 6, except that the modified fluororubber-1 is replaced by modified fluororubber-3 in equal amounts.

[0108] Example 9

[0109] A nitrile rubber chemical foaming material and a preparation method thereof. The specific implementation method is the same as that of Example 6, except that an equal amount of modified fluororubber-1 is replaced by fluororubber.

[0110] Comparative Example 1

[0111] A nitrile rubber chemical foaming material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified nitrile rubber-1 is replaced by nitrile rubber.

[0112] Performance Testing

[0113] The performance of the nitrile rubber chemical foaming materials obtained in the above embodiments and comparative examples was tested:

[0114] (1) Density: Use a densitometer to test the density of nitrile rubber chemical foaming materials;

[0115] (2) Brittle temperature: The low-temperature brittle temperature is measured according to GB / T 1682-2014 “Single specimen method for determination of low-temperature brittleness of vulcanized rubber”;

[0116] (3) Oil resistance: The nitrile rubber chemical foam material was cut into dumbbell-shaped specimens with a length of 150 mm and a narrow parallel width of 10 mm, and immersed in 10 g of 903# standard test oil at 150°C for 70 h. The tensile strength change rate of the specimens was tested according to the method specified in GB / T1690-2010: tensile strength change rate = (tensile strength after immersion - tensile strength before immersion) / tensile strength before immersion × 100%.

[0117] The test results are shown in Table 1:

[0118] Table 1

[0119] Group <![CDATA[Density / g·cm -3 > Brittle temperature / ℃ Change rate of tensile length / % Example 1 0.49 -43.3 -4.2 Example 2 0.52 -41.8 -4.7 Example 3 0.50 -42.5 -4.3 Example 4 0.54 -39.1 -6.5 Example 5 0.53 -40.7 -5.7 Example 6 0.42 -49.1 -3.5 Example 7 0.47 -47.2 -4.3 Example 8 0.46 -46.5 -4.7 Example 9 0.57 -38.6 -5.9 Comparative Example 1 0.62 -35.2 -8.3

[0120] As shown in Table 1, the chemical foaming materials of acrylonitrile-butadiene rubber in Examples 1-3 of the present invention have lower density and better oil resistance and low temperature resistance. By comparing Example 4 with Example 1, it can be seen that by changing the proportion of acetic acid, the introduction of epoxy groups affects the content of double bond groups in the system, thereby affecting the vulcanization effect of acrylonitrile-butadiene rubber, and reducing the low temperature resistance and oil resistance of acrylonitrile-butadiene rubber. By comparing Example 5 with Example 1, it can be seen that changing the proportion of bromo-tetraethylene glycol-carboxylic acid can cause the residual part of the acidic groups to break the molecular chain of acrylonitrile-butadiene rubber, and deteriorate the low temperature resistance and oil resistance of the chemical foaming materials of acrylonitrile-butadiene rubber. By comparing Example 6 with Example 1, it can be seen that adding the modified After the fluororubber is modified, the various properties of the rubber are further improved; from the comparison between Example 7 and Example 6, it can be seen that by changing the ratio of acrylic acid, the residual carboxyl group in the system is not enough to play the role of the blowing agent, so that the density of the nitrile rubber chemical foaming material is increased; from the comparison between Example 8 and Example 6, it can be seen that by changing the ratio of polypropylene glycol, the residual polyether in the system is not enough to play the role of stabilizing the bubbles, so that the density of the nitrile rubber chemical foaming material is increased; from the comparison between Example 9 and Example 6, it can be seen that without modifying the fluororubber, the compatibility of fluororubber and nitrile rubber is not good, resulting in the deterioration of various properties of the rubber; from the comparison between Comparative Example 1 and Example 1, it can be seen that without modifying the nitrile rubber, the various properties of the rubber are not good.

[0121] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A nitrile rubber chemical foaming material, characterized in that: The invention comprises the following raw materials in parts by weight: 40-50 parts of modified nitrile rubber, 1-3 parts of vulcanizing agent, 1-5 parts of vulcanization accelerator, 1-3 parts of activating agent, 1-3 parts of foaming agent, 10-20 parts of calcium carbonate and 2-4 parts of antioxidant.

2. The nitrile rubber chemical foaming material according to claim 1, characterized in that The preparation method of the modified nitrile rubber comprises the following steps: A1, adding nitrile rubber and chlorobenzene to a reaction vessel, stirring at room temperature until the nitrile rubber is dissolved, adding acetic acid and 66-70wt% aqueous hydrogen peroxide solution, heating to 55-65°C for reaction for 5-7h, cooling to room temperature, adding ethanol and stirring for 20-30min, taking out the precipitate, and drying to obtain epoxidized nitrile rubber; A2. Add the epoxidized nitrile rubber and chlorobenzene obtained in step A1 into a reaction vessel, stir at room temperature until the epoxidized nitrile rubber is dissolved, then add brominated-tetraethylene glycol-carboxylic acid and ferric bromide, heat to 120-140 ° C and react for 3-5 hours, cool to room temperature, add ethanol and stir for 20-30 minutes, take out the precipitate, and obtain modified nitrile rubber after drying.

3. The nitrile rubber chemical foaming material according to claim 2, characterized in that In the step A1, the weight ratio of the nitrile rubber, acetic acid and 66-70 wt % aqueous hydrogen peroxide solution is 1:(0.15-0.2):(0.8-1).

4. The nitrile rubber chemical foaming material according to claim 2, characterized in that In the step A2, the weight ratio of the epoxidized nitrile rubber to the brominated-tetraethylene glycol-carboxylic acid is 1:(0.05-0.1).

5. The nitrile rubber chemical foaming material according to claim 1, characterized in that: The foaming agent is diisopropyl azodicarboxylate and sodium bicarbonate, and the weight ratio of the two is 1:(0.4-0.6).

6. The nitrile rubber chemical foaming material according to claim 1, characterized in that: The nitrile rubber chemical foaming material also contains 10-20 parts by weight of modified fluororubber.

7. The nitrile rubber chemical foaming material according to claim 6, characterized in that: The preparation method of the modified fluororubber comprises the following steps: B1. Add acrylic acid, fluororubber and benzoyl peroxide into a reaction vessel, and react at 70-80° C. for 2-4 hours to obtain acrylic acid-modified fluororubber; B2. Add the acrylic modified fluororubber, polyether and phosphoric acid obtained in step B1 into a reaction vessel, heat to 70-80° C. and react for 2-4 hours to obtain modified fluororubber.

8. The nitrile rubber chemical foaming material according to claim 7, characterized in that: The weight ratio of acrylic acid to fluororubber in step B1 is (0.04-0.06):

1.

9. The nitrile rubber chemical foaming material according to claim 7, characterized in that: The weight ratio of acrylic modified fluororubber to polyether in step B2 is 1:(0.1-0.3).

10. A method for preparing the nitrile rubber chemical foaming material according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) placing the modified nitrile rubber in an open mill for plasticizing at a temperature of 70-80° C. for a plasticizing time of 1-2 h to obtain a plasticized rubber; (2) pouring the plasticized rubber obtained in step (1), the vulcanizing agent, the vulcanization accelerator, the activator, the foaming agent, the calcium carbonate, and the antioxidant into an open mill at the same time, and rolling them together until the rubber material is coated with the roller without a viscous liquid on the surface, and then leaving the rolls for 2 to 3 days to form, thereby obtaining a formed rubber; (3) vulcanizing and foaming the molded rubber obtained in step (2) in a flat vulcanizer to obtain the nitrile rubber chemical foaming material, wherein the vulcanization temperature is 165-170° C. and the vulcanization time is 10-20 min.

Citation Information

Cited By

  • Wide-temperature-range anti-gas-explosion hydrogenated nitrile rubber sealing material and preparation method thereof

    CN120310176A

  • Hydrogenated nitrile rubber sealing material with wide temperature range and anti-gas explosion and preparation method thereof

    CN120310176B