Oil-resistant, corrosion-resistant and static-conductive polyurea coating as well as preparation method and application thereof
By using the composition and preparation method of polyurea coating on the inner wall of crude oil storage tank, the problems of poor oil resistance and corrosion resistance of existing coatings are solved, and efficient oil resistance and corrosion resistance and electrostatic conduction effects are achieved, which is suitable for large-scale industrial applications.
Patent Information
- Application Number
- CN202411110845.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing water-based/solvent-based anti-corrosion electrostatic conductive epoxy coatings have poor oil resistance and corrosion resistance on the inner wall of crude oil storage tanks, and the construction process is complicated and cannot meet the practical application requirements.
A polyurea coating that is resistant to oil, corrosion and static electricity is used, and its composition includes polyaspartic acid ester resin, fluorine-containing polyamine resin, anti-rust filler, conductive filler, etc., and high density is formed through specific ratios and preparation methods. A medium-resistant paint film is suitable for forming a protective layer with a larger thickness at one time.
It achieves efficient oil resistance, corrosion resistance and electrostatic conduction effect, and is suitable for protection of the inner wall of crude oil storage tanks, with high construction efficiency and is suitable for large-scale industrial production and application.
Smart Images

Figure CN118931340A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal anticorrosion, and in particular to an oil-resistant, anticorrosive, and static-conductive polyurea coating, and a preparation method and application thereof. Background Art
[0002] Crude oil storage tanks are essential infrastructure for the oil industry, and their main material is metal. Crude oil contains inorganic salts, organic salts, water and other components, which can cause electrochemical corrosion to crude oil storage tanks. Severe corrosion can cause oil leakage. Oil leakage will not only seriously pollute the ecological environment, but also easily cause fires and explosions, posing a great threat to people's lives and safety. In addition, liquid oil will generate static charges due to friction during the flow, filtration, and extraction of liquid oil in the tank, which poses a risk of static fire and explosion. At present, the main method of protection is to coat the inner wall of the crude oil storage tank with water-based / solvent-based anti-corrosion and anti-static epoxy coatings. However, the existing water-based / solvent-based anti-corrosion and anti-static epoxy coatings generally have problems such as general oil resistance and insufficient anti-corrosion effect (the protection period is generally only about 3 years), and there are also many construction processes (the thickness of the paint film formed by a single brushing is only about 50μm, and it is necessary to repeat the brushing multiple times to achieve the appropriate paint film thickness), which cannot fully meet the actual application requirements.
[0003] Therefore, it is of great significance to develop an anti-corrosion coating with excellent oil resistance, excellent anti-corrosion performance, good static conductivity, and a thick paint film formed by one application. Summary of the invention
[0004] The purpose of the present invention is to provide an oil-resistant, corrosion-resistant and static-conducting polyurea coating and a preparation method and application thereof.
[0005] The technical solution adopted by the present invention is:
[0006] An oil-resistant, anti-corrosion and static-conducting polyurea coating comprises the following components in parts by weight:
[0007] Component A:
[0008] Polyaspartic acid ester resin: 40 to 60 parts;
[0009] Fluorine-containing polyamine resin: 3 to 10 parts;
[0010] Anti-rust pigment filler: 5 to 10 parts;
[0011] Conductive filler: 18 to 25 parts;
[0012] Dispersant: 0.4 to 1 part;
[0013] Defoaming agent: 0.3 to 1.2 parts;
[0014] Leveling agent: 0.3 to 0.8 parts;
[0015] Rheological additive: 0.5 to 1.5 parts;
[0016] Diluent: 2 to 5 parts;
[0017] Dewatering agent: 3 to 7 parts;
[0018] Component B:
[0019] Aliphatic isocyanate curing agent: 94 to 98 parts;
[0020] Diluent: 2 to 5 parts.
[0021] Preferably, the polyaspartic acid resin is compounded by polyaspartic acid resin F520 of Shenzhen Feiyang Junyan New Materials Co., Ltd. and polyaspartic acid resin F420 of Shenzhen Feiyang Junyan New Materials Co., Ltd. at a mass ratio of 1.5 to 4.5:1.
[0022] Preferably, the fluorine-containing polyamine resin is prepared by a preparation method comprising the following steps:
[0023] a) dispersing a polyamine in a solvent, and then adding a fluorine-containing carboxylic acid ester to react to obtain a fluorine-containing polyamine intermediate;
[0024] b) adding the fluorine-containing polyamine intermediate into a reducing agent solution for reaction to obtain a fluorine-containing polyamine resin.
[0025] Further preferably, the fluorine-containing polyamine resin is prepared by a preparation method comprising the following steps:
[0026] a) dispersing a polyamine in a solvent, slowly adding a fluorinated carboxylic acid ester to react, and then performing reduced pressure distillation to remove impurities to obtain a fluorinated polyamine intermediate;
[0027] b) dissolving the fluorine-containing polyamine intermediate with a solvent, then slowly adding it to a reducing agent solution for reaction, filtering, and taking the filtrate for rotary evaporation to remove impurities, thereby obtaining a fluorine-containing polyamine resin.
[0028] Preferably, in step a), the molar ratio of the polyamine to the fluorinated carboxylic acid ester is 1:2.5-3.0.
[0029] Preferably, the polyamine in step a) is at least one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, N-(2-ethylamino)-1,3-propylenediamine, N,N'-bis(2-aminoethyl)-1,3-propylenediamine, N,N'-bis(3-aminopropyl)ethylenediamine and N,N'-bis(3-aminopropyl)-1,3-propylenediamine.
[0030] Preferably, the solvent in step a) is methanol.
[0031] Preferably, the fluorine-containing carboxylic acid ester in step a) is at least one of methyl heptafluorobutyrate, ethyl heptafluorobutyrate, methyl nonafluorovalerate, ethyl nonafluorovalerate, methyl undecanoate, ethyl perfluorooctanoate, and ethyl heptadecafluorononanoate.
[0032] Preferably, the reaction in step a) is carried out at a temperature of 30°C to 90°C.
[0033] Preferably, the solvent in step b) is tetrahydrofuran.
[0034] Preferably, the molar ratio of the amide group to the reducing agent in the fluorine-containing polyamine intermediate in step b) is 1:2-3.
[0035] Preferably, the reducing agent in step b) is at least one of lithium aluminum hydride, tetrahydrofuran borane complex and sodium borohydride.
[0036] Preferably, the reaction in step b) is carried out at a temperature of 5°C to 80°C, and the reaction time is 4h to 48h.
[0037] Preferably, the anti-rust pigment filler is at least one of aluminum tripolyphosphate, aluminum zinc phosphate, molybdate, and zinc phosphate.
[0038] Preferably, the conductive filler is conductive mica powder.
[0039] Further preferably, the conductive filler is at least one of the conductive mica powder BC-P of Shanghai Junjiang Technology Co., Ltd., the conductive mica powder BC-C of Shanghai Junjiang Technology Co., Ltd., the conductive mica powder BC-C10 of Shanghai Junjiang Technology Co., Ltd., and the conductive mica powder of Guangzhou Yiji Technology Co., Ltd.
[0040] Preferably, the dispersant is a polyurethane polymer dispersant. The polyurethane polymer dispersant has excellent pigment stability and low temperature stability.
[0041] Preferably, the defoamer is an organosilicon defoamer, which not only has good anti-foaming ability, but also can quickly eliminate bubbles in the coating system, especially has excellent ability to break reactive bubbles.
[0042] Preferably, the leveling agent is fluorocarbon modified polyacrylate. Fluorocarbon modified polyacrylate can significantly reduce the surface tension of the coating, prevent cratering, and help enhance the adhesion of the paint film.
[0043] Preferably, the rheological additive is micronized polyamide modified hydrogenated castor oil. Micronized polyamide modified hydrogenated castor oil can promote the coating system to establish a three-dimensional structure, and the formed thixotropic fluidity can prevent sedimentation and improve anti-sagging performance without affecting the leveling of the coating.
[0044] Preferably, the diluent is an ether ester solvent.
[0045] More preferably, the diluent is at least one of n-butyl acetate, propyl carbonate, diisoamyl methyl phosphate and diisononyl phthalate.
[0046] Preferably, the dehydrating agent is a molecular sieve.
[0047] Preferably, the aliphatic isocyanate curing agent is at least one of hexamethylene diisocyanate trimer, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and methylcyclohexyl diisocyanate.
[0048] A method for preparing the oil-resistant, anti-corrosion and static-conducting polyurea coating as described above comprises the following steps:
[0049] 1) Mixing polyaspartic acid ester resin and fluorine-containing polyamine resin, adding dispersant, defoamer and leveling agent and mixing, adding anti-rust pigment filler and conductive filler and mixing, adding rheological additive, diluent and dewatering agent and mixing to obtain component A, and mixing aliphatic isocyanate curing agent and diluent as component B;
[0050] 2) Mix component A and component B to obtain the oil-resistant, anti-corrosion and anti-static polyurea coating.
[0051] Preferably, a method for preparing the oil-resistant, anti-corrosion and static-conducting polyurea coating as described above comprises the following steps:
[0052] 1) Add polyaspartic acid ester resin and fluorine-containing polyamine resin to a stirrer, stir and disperse for 5 min to 10 min at a stirrer speed of 800 rpm to 1500 rpm, then add dispersant, defoamer and leveling agent, continue to stir and disperse for 5 min to 10 min, then add anti-rust color filler and conductive filler, adjust the stirrer speed to 2500 rpm to 3000 rpm and stir and disperse for 15 min to 20 min, then add rheological additive, diluent and dewatering agent, adjust the stirrer speed to 1200 rpm to 1700 rpm and stir and disperse for 10 min to 15 min to obtain component A, and mix aliphatic isocyanate curing agent and diluent as component B;
[0053] 2) Mix component A and component B to obtain the oil-resistant, anti-corrosion and anti-static polyurea coating.
[0054] The oil-resistant, anti-corrosion and electrostatically conductive polyurea coating as described above is used for metal corrosion protection.
[0055] The beneficial effects of the present invention are as follows: the polyurea coating of the present invention can form a thick paint film after one application, the construction efficiency is high, the paint film has excellent oil resistance, excellent anti-corrosion performance, good static electricity conductive effect, and excellent mechanical properties, and is suitable for use as an inner wall protective coating for crude oil storage tanks. The preparation method of the polyurea coating is simple, and is suitable for large-scale industrial production and application.
[0056] Specifically:
[0057] 1) The polyurea coating of the present invention contains a fluorine-containing polyamine resin, which can increase the crosslinking density of the paint film, which is beneficial to enhancing the salt spray resistance and acid and alkali resistance of the paint film, thereby improving the corrosion resistance of the paint film, and the fluorocarbon chain in the fluorine-containing polyamine resin is beneficial to improving the oil resistance of the paint film;
[0058] 2) During the curing process of the polyurea coating of the present invention, the aliphatic isocyanate curing agent reacts with the polyaspartic acid ester resin and the fluorine-containing polyamine resin to generate urea groups that can form hydrogen bonds, forming a microscopic phase separation structure at the molecular level, thereby giving the paint film excellent mechanical properties;
[0059] 3) The paint film formed by the polyurea coating of the present invention has excellent medium resistance, for example, solvent resistance (93# gasoline 62°C), salt spray resistance, salt resistance (5% NaCl solution, room temperature), alkali resistance (5% NaOH solution, room temperature) and acid resistance (5% H2SO4 solution, room temperature) can all reach more than 1500 hours, and boiling water resistance can also reach more than 50 hours, which fully meets the requirements for corrosion protection of steel crude oil storage tanks;
[0060] 4) The polyurea coating of the present invention contains conductive fillers, and the paint film has a good static conductive effect, which can effectively avoid the problem of fire and explosion caused by static electricity;
[0061] 5) The fluorine-containing polyamine resin in the polyurea coating of the present invention is prepared by a two-step method, the reaction conditions are simple, and the yield of the product is high;
[0062] 6) The ratio of the fluorine-containing polyamine resin, the polyaspartic acid ester resin and the aliphatic isocyanate curing agent in the polyurea coating of the present invention is appropriate, the activation period of the coating and the hardness of the paint film can be flexibly adjusted, and the thickness of the paint film formed by the coating in one application can reach tens of microns to hundreds of microns. The required paint film thickness can be obtained in one application, which significantly improves the construction efficiency;
[0063] 7) The preparation method of the polyurea coating of the present invention is simple and suitable for large-scale industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Figure 1 This is a high-resolution mass spectrum of the fluorinated polyamine intermediate in Example 1.
[0065] Figure 2 This is a high-resolution mass spectrum of the fluorine-containing polyamine resin in Example 1. DETAILED DESCRIPTION
[0066] The present invention will be further explained and illustrated below in conjunction with specific embodiments.
[0067] Embodiment 1:
[0068] An oil-resistant, anti-corrosion and electrostatically conductive polyurea coating, the composition of which is shown in the following table:
[0069] Table 1 Composition of an oil-resistant, anti-corrosion and electrostatically conductive polyurea coating
[0070]
[0071] Note:
[0072] The preparation method of fluorine-containing polyamine resin is as follows:
[0073] a) 15.9 g of tetraethylenepentamine and 7 g of methanol were stirred evenly, and then the temperature was raised to 45° C. and 40 g of methyl heptafluorobutyrate was added dropwise to react, and the reaction progress was monitored by thin layer chromatography analysis. After the reaction was completed, impurities were removed by vacuum distillation to obtain a fluorine-containing polyamine intermediate;
[0074] b) 30 g of the fluorinated polyamine intermediate was dissolved in 6 g of tetrahydrofuran, and then added dropwise to 260 mL of a 1 mol / L lithium aluminum hydride tetrahydrofuran solution. After the addition was complete, the temperature was raised to 35° C. and the reaction was carried out for 24 h. After the reaction was completed, 9.9 g of deionized water, 9.9 g of a 15% NaOH solution, and 30 g of deionized water were used for post-treatment in sequence, and anhydrous magnesium sulfate was added to remove water, filtered, and the filtrate was subjected to rotary evaporation to remove impurities to obtain a fluorinated polyamine resin.
[0075] The high resolution mass spectrum (HR-MS) of the fluorinated polyamine intermediate in this example is shown in FIG. Figure 1 As shown, the HR-MS diagram of fluorinated polyamine resin is as follows Figure 2 shown.
[0076] Depend on Figure 1 and Figure 2 It can be seen that the fluorine-containing polyamine resin was successfully prepared in this embodiment, and according to the signal intensity of the mass spectrometer, the content of the target product in the synthesized product was high and the reaction yield was large.
[0077] The preparation method of the above-mentioned oil-resistant, anti-corrosion and static-conducting polyurea coating is as follows:
[0078] 1) Add polyaspartic acid resin F520, polyaspartic acid resin F420 and fluorine-containing polyamine resin into a mixer, stir and disperse for 10 minutes at a mixer speed of 1200 rpm, then add dispersant AFCONA-4071, defoamer AFCONA2605-5B, defoamer 768 and leveling agent AFCONA-3670, continue to stir and disperse for 10 minutes, then add aluminum tripolyphosphate and conductive mica powder, adjust the mixer speed to 2500 rpm, stir and disperse for 20 minutes, and then add rheological additive MT, n-butyl acetate and 3A molecular sieve, adjust the speed of the stirrer to 1500rpm and stir and disperse for 12 minutes to obtain component A; stir hexamethylene diisocyanate trimer TPA-100, isophorone diisocyanate and n-butyl acetate to obtain component B;
[0079] 2) Component A and component B are mixed evenly according to an NCO index of 1.1 to obtain an oil-resistant, anti-corrosion and anti-static polyurea coating.
[0080] Embodiment 2:
[0081] An oil-resistant, anti-corrosion and anti-static polyurea coating is completely the same as the oil-resistant, anti-corrosion and anti-static polyurea coating in Example 1 except that the fluorine-containing polyamine resin used is different (the addition amount is the same).
[0082] Note:
[0083] The preparation method of fluorine-containing polyamine resin is as follows:
[0084] a) 15.9 g of tetraethylenepentamine and 7 g of methanol were stirred evenly, and then the temperature was raised to 85° C. and 50.4 g of ethyl nonafluoropentanoate was added dropwise to react, and the reaction progress was monitored by thin layer chromatography analysis. After the reaction was completed, impurities were removed by vacuum distillation to obtain a fluorine-containing polyamine intermediate;
[0085] b) 40 g of the fluorinated polyamine intermediate was dissolved in 7 g of tetrahydrofuran, and then added dropwise to 289 mL of a 1 mol / L lithium aluminum hydride tetrahydrofuran solution. After the addition was complete, the temperature was raised to 45° C. and the reaction was carried out for 24 h. After the reaction was completed, 11 g of deionized water, 11 g of a 15% NaOH solution, and 33 g of deionized water were used for post-treatment in sequence, and anhydrous magnesium sulfate was added for dehydration. The mixture was filtered, and the filtrate was subjected to rotary evaporation to remove impurities to obtain a fluorinated polyamine resin.
[0086] Embodiment 3:
[0087] An oil-resistant, anti-corrosion and anti-static polyurea coating is completely the same as the oil-resistant, anti-corrosion and anti-static polyurea coating in Example 1 except that the fluorine-containing polyamine resin used is different (the addition amount is the same).
[0088] Note:
[0089] The preparation method of fluorine-containing polyamine resin is as follows:
[0090] a) 15.9 g of tetraethylene pentamine and 7 g of methanol were stirred evenly, and then the temperature was raised to 80° C. and 42 g of ethyl heptafluorobutyrate was added dropwise to react, and the reaction progress was monitored by thin layer chromatography analysis. After the reaction was completed, impurities were removed by vacuum distillation to obtain a fluorine-containing polyamine intermediate;
[0091] b) 35 g of the fluorinated polyamine intermediate was dissolved in 7 g of tetrahydrofuran, and then added dropwise to 290 mL of a 1 mol / L lithium aluminum hydride tetrahydrofuran solution. After the addition was complete, the temperature was raised to 35° C. and the reaction was carried out for 24 h. After the reaction was completed, 11 g of deionized water, 11 g of a 15% NaOH solution by mass, and 33 g of deionized water were used for post-treatment in sequence, and anhydrous magnesium sulfate was added to remove water, filtered, and the filtrate was subjected to rotary evaporation to remove impurities to obtain a fluorinated polyamine resin.
[0092] Embodiment 4:
[0093] An oil-resistant, anti-corrosion and electrostatically conductive polyurea coating, the composition of which is shown in the following table:
[0094] Table 2 Composition of an oil-resistant, anti-corrosion and electrostatically conductive polyurea coating
[0095]
[0096]
[0097] Embodiment 5:
[0098] An oil-resistant, anti-corrosion and electrostatically conductive polyurea coating, the composition of which is shown in the following table:
[0099] Table 3 Composition of an oil-resistant, anti-corrosion and electrostatically conductive polyurea coating
[0100]
[0101]
[0102] Comparative Example 1:
[0103] A polyurea coating is exactly the same as the oil-resistant, anti-corrosion and anti-static polyurea coating in Example 3, except that the polyaspartic acid ester resin F420 is replaced by the polyaspartic acid ester resin F520 (equal weight replacement) and the fluorine-containing polyamine resin is replaced by the polyaspartic acid ester resin F520 (equal weight replacement).
[0104] Comparative Example 2:
[0105] A polyurea coating is identical to the oil-resistant, anti-corrosion and anti-static polyurea coating in Example 3 except that the polyaspartic acid resin F520 is replaced by the polyaspartic acid resin F420 (equal weight replacement).
[0106] Comparative Example 3:
[0107] A polyurea coating is exactly the same as the oil-resistant, anti-corrosion and anti-static polyurea coating in Example 3, except that component B is replaced by 100 parts by mass of aromatic isocyanate MDI-50 (Wanhua).
[0108] Comparative Example 4:
[0109] Water-based anti-corrosion and static conductive epoxy coating (water-based epoxy static conductive anti-corrosion coating YHW2502 produced by Guangzhou Jitai Chemical Co., Ltd.).
[0110] Performance Test:
[0111] 1) The performance comparison table of the polyurea coatings in Example 3 and Comparative Examples 1 to 3 is shown in the following table:
[0112] Table 4 Performance comparison of polyurea coatings in Example 3 and Comparative Examples 1 to 3
[0113]
[0114]
[0115] Note:
[0116] Preparation process of paint film: Use a scraper to scrape the paint sample onto the steel plate, control the thickness of the paint film to 250μm~350μm, and cure at room temperature for 7 days to obtain the paint film.
[0117] Surface drying time and actual drying time: Tested in accordance with "GB / T 1728-2020 Determination of drying time of paint film and putty film";
[0118] Flexibility: Tested in accordance with "GB / T 1731-2020 Determination of flexibility of paint film and putty film";
[0119] Impact resistance: Tested in accordance with "GB / T 1732-2020 Determination of impact resistance of paint film";
[0120] Adhesion: Tested in accordance with "GB / T 9286-2021 Paint and varnish cross-cut test";
[0121] Pencil hardness: Test according to "GB / T 6739-2022 Paints and varnishes - Pencil method for determination of film hardness";
[0122] Boiling water resistance: Tested in accordance with "GB / T 1733-1993 Determination of water resistance of paint film";
[0123] Gasoline resistance: Tested in accordance with "SY / T 0319-2012 Technical Standard for Internal Anticorrosion Layer of Liquid Coatings for Steel Storage Tanks";
[0124] Acid resistance, alkali resistance and salt resistance: Tested in accordance with Method A of "GB / T 9274-1988 Determination of resistance of paints and varnishes to liquid media";
[0125] Salt spray resistance: Tested in accordance with "GB / T 1771-2007 Determination of neutral salt spray resistance of paints and varnishes";
[0126] Index value: Performance index of electrostatically conductive anti-corrosion coatings in "GB / T 50393-2017 Technical Standard for Anti-Corrosion Engineering of Steel Petroleum Storage Tanks".
[0127] From Table 4, we can see that:
[0128] a) The resin component of the polyurea coating in Comparative Example 1 is only polyaspartic acid ester resin F520, which has low reactivity, so the paint film cures too slowly and foams severely, resulting in poor density of the paint film and poor medium resistance;
[0129] b) The resin components of the polyurea coating in Comparative Example 2 are polyaspartic acid ester resin F420 and fluorine-containing polyamine resin. Since the reaction speed of F420 is too fast, the coating cannot be applied to the substrate, so the practical value of the formula is low;
[0130] c) Component B of the polyurea coating in Comparative Example 3 is an aromatic curing agent MDI-50, which has high reactivity and a much higher reaction rate with water than aliphatic isocyanates TPA-100 and IPDI, resulting in obvious foaming of the paint film, reduced density of the paint film, and thus poor medium resistance;
[0131] d) The polyurea coating in Example 1 is added with a fluorinated polyamine resin. The multifunctional amine group can increase the crosslinking density of the paint film, thereby improving the media resistance of the paint film. The fluorinated chain segment is also beneficial to improving the oil and media resistance of the paint film. The appropriate ratio of polyaspartic acid resin F520 / F420 can provide a suitable activation period. The curing agent can not only adjust the activation period and expand the selection range of construction equipment by mixing aliphatic isocyanates, but also improve the media resistance of the paint film.
[0132] 2) The performance comparison table of the polyurea coatings in Examples 1 to 5 and the epoxy coating in Comparative Example 4 is shown in the following table:
[0133] Table 5 Performance comparison of polyurea coatings in Examples 1 to 5 and epoxy coatings in Comparative Example 4
[0134]
[0135]
[0136] Note:
[0137] Preparation process of paint film: Use a scraper to scrape the paint sample onto the steel plate, control the thickness of the paint film to 250μm~350μm, and cure at room temperature for 7 days to obtain the paint film.
[0138] Surface resistivity: Tested in accordance with "GB / T 31838.3-2019 Dielectric and resistance properties of solid insulating materials Part 3: Resistance characteristics (DC method) Surface resistance and surface resistivity";
[0139] Adhesion: Test according to "GB / T 5210-2006 Paint and varnish adhesion test by pull-off method".
[0140] From Table 5, we can see that:
[0141] a) The polyurea coatings in Examples 1 to 5 (added with fluorinated polyamine resin) are compared with the epoxy coating in Comparative Example 4. The acid resistance, alkali resistance, salt resistance, salt spray resistance and gasoline resistance of the paint film can reach more than 1500 hours, and the boiling water resistance can reach more than 60 hours, and the corrosion resistance and oil resistance are more excellent;
[0142] b) The surface resistivity of the paint films formed by the polyurea coatings in Examples 1 to 5 are all within the specified range, and have excellent electrostatic conductivity;
[0143] c) The dry film thickness of the epoxy coating in Comparative Example 4 is only 40 μm to 60 μm after one spraying, and multiple sprayings are required to reach the specified thickness of 250 μm to 350 μm. However, due to the high solid content of the polyurea coatings in Examples 1 to 5, the dry film thickness can reach the specified thickness of 250 μm to 350 μm after one spraying, which significantly improves the construction efficiency;
[0144] In summary, the oil-resistant, anti-corrosion and anti-static polyurea coating of the present invention has high construction efficiency and low time cost, and the formed paint film has excellent oil resistance, anti-corrosion and anti-static properties.
[0145] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. An oil-resistant, anti-corrosion and electrostatically conductive polyurea coating, characterized in that: The composition comprises the following components in parts by weight: Component A: Polyaspartic acid ester resin: 40 to 60 parts; Fluorine-containing polyamine resin: 3 to 10 parts; Anti-rust pigment filler: 5 to 10 parts; Conductive filler: 18 to 25 parts; Dispersant: 0.4 to 1 part; Defoaming agent: 0.3 to 1.2 parts; Leveling agent: 0.3 to 0.8 parts; Rheological additive: 0.5 to 1.5 parts; Diluent: 2 to 5 parts; Dewatering agent: 3 to 7 parts; Component B: Aliphatic isocyanate curing agent: 94 to 98 parts; Diluent: 2 to 5 parts.
2. The oil-resistant, anti-corrosion and anti-static polyurea coating according to claim 1, characterized in that: The fluorine-containing polyamine resin is prepared by a preparation method comprising the following steps: a) dispersing a polyamine in a solvent, and then adding a fluorine-containing carboxylic acid ester to react to obtain a fluorine-containing polyamine intermediate; b) adding the fluorine-containing polyamine intermediate into a reducing agent solution for reaction to obtain a fluorine-containing polyamine resin.
3. The oil-resistant, anti-corrosion and anti-static polyurea coating according to claim 2, characterized in that: The molar ratio of the polyamine to the fluorinated carboxylic acid ester in step a) is 1:2.5-3.0; the molar ratio of the amide group in the fluorinated polyamine intermediate to the reducing agent in step b) is 1:2-3.
4. The oil-resistant, anti-corrosion and anti-static polyurea coating according to claim 2, characterized in that: The polyamine in step a) is at least one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, N-(2-ethylamino)-1,3-propylenediamine, N,N'-bis(2-aminoethyl)-1,3-propylenediamine, N,N'-bis(3-aminopropyl)ethylenediamine, and N,N'-bis(3-aminopropyl)-1,3-propylenediamine; the fluorine-containing carboxylic acid ester in step a) is at least one of methyl heptafluorobutyrate, ethyl heptafluorobutyrate, methyl nonafluorovalerate, ethyl nonafluorovalerate, methyl undecanoate, ethyl perfluorooctanoate, and ethyl heptadecafluorononanoate; the reducing agent in step b) is at least one of lithium aluminum hydride, tetrahydrofuran borane complex, and sodium borohydride.
5. The oil-resistant, anti-corrosion and static-conducting polyurea coating according to claim 2, characterized in that: The reaction in step a) is carried out at a temperature of 30°C to 90°C; the reaction in step b) is carried out at a temperature of 5°C to 80°C, and the reaction time is 4h to 48h.
6. The oil-resistant, anti-corrosion and anti-static polyurea coating according to any one of claims 1 to 5, characterized in that: The anti-rust pigment filler is at least one of aluminum tripolyphosphate, aluminum zinc phosphate, molybdate, and zinc phosphate; and the conductive filler is conductive mica powder.
7. The oil-resistant, anti-corrosion and anti-static polyurea coating according to any one of claims 1 to 5, characterized in that: The dispersant is a polyurethane polymer dispersant; the defoamer is an organosilicon defoamer; the leveling agent is a fluorocarbon modified polyacrylate; the rheological additive is a micronized polyamide modified hydrogenated castor oil; the diluent is an ether ester solvent; and the dewatering agent is a molecular sieve.
8. The oil-resistant, anti-corrosion and anti-static polyurea coating according to any one of claims 1 to 5, characterized in that: The aliphatic isocyanate curing agent is at least one of hexamethylene diisocyanate trimer, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and methylcyclohexyl diisocyanate.
9. A method for preparing the oil-resistant, anti-corrosion and static-conducting polyurea coating according to any one of claims 1 to 8, characterized in that: The following steps are involved: 1) Mixing polyaspartic acid ester resin and fluorine-containing polyamine resin, adding dispersant, defoamer and leveling agent and mixing, adding anti-rust pigment filler and conductive filler and mixing, adding rheological additive, diluent and dewatering agent and mixing to obtain component A, and mixing aliphatic isocyanate curing agent and diluent as component B; 2) Mix component A and component B to obtain the oil-resistant, anti-corrosion and anti-static polyurea coating.
10. Use of the oil-resistant, anti-corrosion and electrostatically conductive polyurea coating as claimed in any one of claims 1 to 8 for metal corrosion protection.
Citation Information
Patent Citations
Fluorine modified aspartic polyurea coating and preparation method thereof
CN109207039A
Anticorrosive static-conductive solvent-free polyurea coating as well as preparation method and application thereof
CN114149729A
Self-cleaning type anti-corrosion weather-resistant polyurea coating
CN114644877A
Method of producing fluorine-containing aliphatic amine
JP2015178492A
Cited By
Water-based anticorrosive paint for rare earth permanent magnet motor and preparation method of water-based anticorrosive paint