Cold-resistant sheath material and preparation method thereof, cold-resistant marine cable and manufacturing method thereof

By using cold-resistant sheath material and thermoset halogen-free low-smoke polyolefin material, combined with high flame retardant PP low-halogen filler rope and halogen-free low-smoke flame retardant glass fiber tape, the brittle cracking problem of marine cables in extremely low temperature environments is solved. It improves the cold resistance, flame retardant and mechanical properties of the cable, ensuring the safe navigation of ships in extremely cold areas.

CN119019778APending Publication Date: 2024-11-26ZHONGTIAN TECH IND WIRE&CABLE SYST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411141713.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing marine cables are prone to brittle cracking in extremely low temperature environments, which cannot meet the safe operation needs of ships on polar routes, and lack the performance of fuel oil and mineral oil.

Method used

A cold-resistant sheath material is made of polyolefin powder, modifier, flame retardant, ethylene-vinyl acetate copolymer, ethylene propylene teremer rubber, compatibility agent, antioxidant, lubricant and crosslinking agent. Made and granulated through a twin screw extruder, combining the design of thermoset halogen-free low-smoke polyolefin material and high flame retardant PP low-halogen fill rope and halogen-free low-smoke flame retardant glass fiber tape to form a cold-resistant marine cable.

Benefits of technology

Working normally at an ambient temperature of -60℃, replacing ordinary marine cables, improve the flame retardant performance, low halogen and low smoke performance, flexibility and physical and mechanical properties of the cables, ensuring the safe navigation of the ship in extremely cold areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019778A_ABST
    Figure CN119019778A_ABST
Patent Text Reader

Abstract

The invention relates to a cold-resistant sheath material and a preparation method thereof, a cold-resistant marine cable and a manufacturing method thereof, and the cold-resistant sheath material is prepared from the following raw materials by weight: 30-50 parts of an ethylene-vinyl acetate copolymer; 10 to 20 parts of ethylene propylene diene monomer; 1-2 parts of polyolefin powder; 100 to 130 parts of a flame retardant; 3-5 parts of a modifier; 5-8 parts of a compatilizer; 1-3 parts of an antioxidant; 1.5 to 5 parts of a lubricant; and 1-1.5 parts of a cross-linking agent. The low-temperature-resistant marine cable has good tensile strength, elongation at break, oxygen index and oil resistance, and can normally work at the ambient temperature of-60 DEG C, so that the low-temperature-resistant marine cable replaces a common marine cable and can only resist the application environment with the low temperature of-15 DEG C, safe transmission guarantee is provided for sailing operation of ships in extremely cold areas, and safe use at the extremely low ambient temperature is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cable materials, and in particular to a cold-resistant sheath material and a preparation method thereof, and a cold-resistant shipboard cable and a manufacturing method thereof. Background Art

[0002] With the advancement of globalization, maritime transportation has become an important link connecting various countries and regions. As an important tool for marine development, the safety performance of ships is of vital importance. In order to develop and utilize marine resources, ships need to operate for a long time in various harsh marine environments, which puts higher requirements on the supporting equipment of ships. Therefore, it is necessary to invent new structural materials, marine cables, to meet the safe operation of ships in harsh environments.

[0003] The safe application temperature of existing marine cables is -15℃, which cannot meet the extremely low temperature environment requirements of ships on polar routes. Ordinary marine cables are prone to brittle fracture at low temperatures, resulting in cracks in the insulation layer and sheath layer, affecting the electrical operation safety of the ship. With the increasing requirements for ship safety, new structural marine cold-resistant flame-retardant cables are required to not only have good electrical conductivity, mechanical strength and anti-aging properties, but also be resistant to fuel oil and mineral oil, as well as safe application performance in extremely cold climates with mechanical vibration.

[0004] Therefore, it is necessary to provide a cold-resistant sheath material and a preparation method, a cold-resistant shipboard cable and a manufacturing method that can ensure safe use at extremely low ambient temperatures. Summary of the invention

[0005] In order to overcome the deficiencies of the prior art, the present invention provides a cold-resistant sheath material and a preparation method thereof, a cold-resistant shipboard cable and a manufacturing method thereof.

[0006] The technical solution of the present invention is as follows:

[0007] A cold-resistant sheath material is made from the following raw materials in parts by weight:

[0008]

[0009]

[0010] As a further improvement of the present invention, the flame retardant is aluminum hydroxide, and the compatibilizer is maleic anhydride grafted ethylene vinyl acetate.

[0011] A method for preparing a cold-resistant sheath material, the preparation method comprising:

[0012] S1: Mix polyolefin powder and modifier evenly according to proportion;

[0013] S2: adding flame retardant to the mixture and adding it to a high-speed mixer for high-speed stirring;

[0014] S3: adding ethylene-vinyl acetate copolymer, ethylene propylene diene monomer rubber, compatibilizer, antioxidant, lubricant and cross-linking agent into the mixture according to the formula ratio, and placing the mixture into a high-speed mixer for low-speed stirring;

[0015] S4: putting the mixture into a twin-screw extruder for extrusion granulation and drying.

[0016] As a further improvement of the present invention, in step S2, the temperature of the high-speed stirring is 40-45°C.

[0017] As a further improvement of the present invention, in step S3, the low-speed stirring time is 4-6 minutes.

[0018] As a further improvement of the present invention, in step S4, the extrusion temperature of the granulation is 180°C and the drying temperature is 85°C.

[0019] A cold-resistant shipboard cable comprises a cable core, a cabling wrapping tape, an inner sheath, an armor layer, an armor outer protection tape and an outer sheath which are arranged in sequence from the inside to the outside. The outer sheath is made of the above-mentioned cold-resistant sheath material. The cable core comprises a plurality of twisted cores. Cabling filling materials are arranged between the cores and between the cores and the cabling wrapping tape. The core comprises a conductor, a conductor wrapping tape wrapped around the outside of the conductor, and an insulating layer coated on the conductor wrapping tape.

[0020] A method for manufacturing a cold-resistant shipboard cable, the manufacturing method comprising:

[0021] T1: Wire drawing and annealing process, the conductor raw material is drawn into a single wire of a set diameter, the single wire is annealed and softened at high temperature, the single wire is cooled in normal temperature water, and then blown dry with compressed air and wired onto the take-up reel;

[0022] T2: Bundling process, the drawn single wires are bundled into conductor units;

[0023] T3: Re-twisting process, the bundled conductor units are re-twisted into conductors, and a layer of conductor wrapping tape is wrapped around the conductors;

[0024] T4: Insulation process, the insulation material is coated on the outside of the conductor wrapping tape, and the molecules of the insulation material are transformed from a linear structure to a mesh structure through steam cross-linking;

[0025] T5: Cabling process, fill the gap with cabling filling material, twist the cable core into a round shape through a cabling and paralleling die, wrap a layer of cabling wrapping tape around the cable core, and wrap a layer of inner sheath around the cabling wrapping tape;

[0026] T6: Braided armor wrapping protection process, the specified number of braided wires are evenly woven outside the inner sheath to form an armor layer, and an armor outer protection belt is wrapped outside the armor layer;

[0027] T7: Outer sheath process, using an extruder to first extrude and melt the above-mentioned cold-resistant sheath material, and then after being shaped by an extrusion die, it is coated on the outside of the armor outer protection belt to form an outer sheath.

[0028] As a further improvement of the present invention, the temperatures of the extruder are: 90-110°C in the feeding section, 140-160°C in the melting section, 170-180°C in the homogenizing section, and 175-185°C in the die head, and the screw compression ratio of the extruder is 1.8-2.

[0029] As a further improvement of the present invention, the diameter of the single wire is 0.25-0.4 mm, the annealing temperature is 500-600° C., and the cross-sectional area of ​​the conductor unit is 1-16 mm 2 , the cross-sectional area of ​​the conductor is 25-400mm 2 .

[0030] As a further improvement of the present invention, the conductor wrapping tape is a non-woven fabric, the nominal thickness of the conductor wrapping tape is 0.16 mm, the overlap rate exceeds 25%, and the wrapping direction is right; the cabling wrapping tape is a halogen-free low-smoke flame-retardant glass fiber tape, the nominal thickness of the cabling wrapping tape is 0.17 mm, the overlap rate exceeds 25%, and the wrapping direction is left; the armor outer protective tape is a non-woven dotted fabric, the nominal thickness of the armor outer protective tape is 0.1 mm, the overlap rate exceeds 25%, and the wrapping direction is left.

[0031] As a further improvement of the present invention, the insulating material is silane cross-linked polyethylene, and the cable filling material is highly flame-retardant PP low-halogen filling rope.

[0032] According to the present invention of the above scheme, the beneficial effects of the present invention are:

[0033] 1. The present invention can work normally at an ambient temperature of -60°C, thus replacing ordinary marine cables that can only withstand low-temperature applications of -15°C, providing safe transmission guarantees for ships sailing in extremely cold areas, and ensuring safe use at extremely low ambient temperatures;

[0034] 2. The present invention adopts thermosetting halogen-free low-smoke polyolefin materials to replace the existing thermoplastic halogen-free low-smoke polyolefin material technology used in low-temperature environments, retaining the mechanical and physical properties of thermoplastic materials, and solving the problem of the relative conflict between the addition ratio of the flame retardant properties and the low-temperature resistance properties of thermosetting halogen-free low-smoke polyolefin materials;

[0035] 3. Under the premise of meeting the low temperature resistance performance, the present invention adopts high flame retardant PP low halogen filling rope and halogen-free low smoke flame retardant glass fiber tape during cabling, thereby improving the flame retardant performance and low halogen and low smoke performance of the cable from the perspective of cable structure and materials;

[0036] 4. The present invention ensures the flexibility of the cable through material selection, conductor process design and production process, so that the cable has an excellent bending radius;

[0037] 5. The present invention achieves excellent physical, mechanical and shielding properties through the selection and process control of armor materials and processes;

[0038] 6. The present invention achieves excellent low temperature resistance and oil resistance by selecting inner and outer sheath materials and optimizing process structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a preparation flow chart of the cold-resistant sheath material of the present invention;

[0040] Figure 2 It is a structural schematic diagram of the cold-resistant shipboard cable of the present invention;

[0041] Figure 3 The present invention is a production flow chart of the cold-resistant shipboard cable.

[0042] In the figure: 1. conductor; 2. conductor wrapping tape; 3. insulation layer; 4. cabling filling material; 5. cabling wrapping tape; 6. inner sheath; 7. armor layer; 8. armor outer protection tape; 9. outer sheath. DETAILED DESCRIPTION

[0043] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0045] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0046] The present invention provides a cold-resistant sheath material, which is made of the following raw materials in parts by weight:

[0047]

[0048] Preferably, the flame retardant is aluminum hydroxide, and the compatibilizer is maleic anhydride grafted ethylene vinyl acetate.

[0049] See also Figure 1 The present invention provides a method for preparing a cold-resistant sheath material, the preparation method comprising:

[0050] S1: Mix polyolefin powder and modifier evenly according to proportion;

[0051] S2: adding flame retardant to the mixture and adding it to a high-speed mixer for high-speed stirring;

[0052] S3: adding ethylene-vinyl acetate copolymer, ethylene propylene diene monomer rubber, compatibilizer, antioxidant, lubricant and cross-linking agent into the mixture according to the formula ratio, and placing the mixture into a high-speed mixer for low-speed stirring;

[0053] S4: putting the mixture into a twin-screw extruder for extrusion granulation and drying.

[0054] The invention has good tensile strength, elongation at break, oxygen index and oil resistance, and can work normally at an ambient temperature of -60°C, thereby replacing ordinary marine cables that can only withstand low-temperature application environments of -15°C, providing safe transmission guarantees for ships sailing in extremely cold areas, and ensuring safe use at extremely low ambient temperatures.

[0055] The present invention provides the following four embodiments:

[0056] Example 1

[0057] Cold-resistant sheath material 1, the formula contains the following components by weight:

[0058]

[0059] Preparation method:

[0060] S1: Mix polyolefin powder and modifier evenly according to proportion;

[0061] S2: adding flame retardant to the mixture, adding it to a high-speed mixer, and stirring at high speed at 40-45°C;

[0062] S3: Add ethylene-vinyl acetate copolymer, EPDM rubber, compatibilizer, antioxidant, lubricant and crosslinking agent to the mixture according to the formula ratio, and put it into a high-speed mixer for low-speed stirring for 4-6 minutes;

[0063] S4: putting the mixture into a twin-screw extruder for extrusion granulation and drying. The extrusion temperature of the granulation is 180°C and the drying temperature is 85°C.

[0064] Example 2

[0065] Cold-resistant sheath material 2, the formula contains the following components by weight:

[0066]

[0067] Preparation method:

[0068] S1: Mix polyolefin powder and modifier evenly according to proportion;

[0069] S2: adding flame retardant to the mixture, adding it to a high-speed mixer, and stirring at high speed at 40-45°C;

[0070] S3: Add ethylene-vinyl acetate copolymer, EPDM rubber, compatibilizer, antioxidant, lubricant and crosslinking agent to the mixture according to the formula ratio, and put it into a high-speed mixer for low-speed stirring for 4-6 minutes;

[0071] S4: putting the mixture into a twin-screw extruder for extrusion granulation and drying. The extrusion temperature of the granulation is 180°C and the drying temperature is 85°C.

[0072] Example 3

[0073] Cold-resistant sheath material 3, the formula comprises the following components in parts by weight:

[0074]

[0075]

[0076] Preparation method:

[0077] S1: Mix polyolefin powder and modifier evenly according to proportion;

[0078] S2: adding flame retardant to the mixture, adding it to a high-speed mixer, and stirring at high speed at 40-45°C;

[0079] S3: Add ethylene-vinyl acetate copolymer, EPDM rubber, compatibilizer, antioxidant, lubricant and crosslinking agent to the mixture according to the formula ratio, and put it into a high-speed mixer for low-speed stirring for 4-6 minutes;

[0080] S4: putting the mixture into a twin-screw extruder for extrusion granulation and drying. The extrusion temperature of the granulation is 180°C and the drying temperature is 85°C.

[0081] Example 4

[0082] Cold-resistant sheath material 4, the formula comprises the following components in parts by weight:

[0083]

[0084] Preparation method:

[0085] S1: Mix polyolefin powder and modifier evenly according to proportion;

[0086] S2: adding flame retardant to the mixture, adding it to a high-speed mixer, and stirring at high speed at 40-45°C;

[0087] S3: Add ethylene-vinyl acetate copolymer, EPDM rubber, compatibilizer, antioxidant, lubricant and crosslinking agent to the mixture according to the formula ratio, and put it into a high-speed mixer for low-speed stirring for 4-6 minutes;

[0088] S4: putting the mixture into a twin-screw extruder for extrusion granulation and drying. The extrusion temperature of the granulation is 180°C and the drying temperature is 85°C.

[0089] The above four embodiments are compared with the components of existing materials, and the results are as follows:

[0090] Components Example 1 Example 2 Example 3 Example 4 Existing Materials Ethylene-vinyl acetate copolymer 30 servings 50 servings 35 servings 40 servings 40 servings EPDM 10 servings 20 servings 18 servings 15 servings / Low density polyethylene / / / / 14 servings Polyolefin elastomer / / / / 16 servings Polyolefin powder 1 serving 2 servings 1.3 servings 1.5 servings / Flame retardants 100 copies 130 copies 110 copies 115 copies 18 servings Modifier 3 servings 5 servings 4 servings 4 servings 4 servings Compatibilizer 5 servings 8 servings 7 servings 6.5 servings 6 servings Antioxidants 1 serving 3 servings 2.5 servings 2 servings 1.3 servings Lubricants 1.5 servings 5 servings 4.5 servings 3 servings 3 servings Crosslinking agent 1 serving 1.5 servings 1.3 servings 1.3 servings 1.5 servings

[0091] The performance of the above four embodiments is compared and analyzed with the existing materials, and the results are as follows:

[0092]

[0093]

[0094] The properties of Example 3 manufactured according to the above formula are as follows: tensile strength 13.5 MPa, elongation at break 240%, oxygen index 32%, density 1.52 g / cm 3 , volume resistivity 5.8×10 13Ω.m, after the sample is immersed in IRM902 oil at 100℃×24h, the change rate of tensile strength and elongation at break are ≤±40%, and it passes the low-temperature impact embrittlement test at -60℃ with the failure number of 0 / 30, and has excellent low-temperature resistance.

[0095] See also Figure 2 The present invention provides a cold-resistant shipboard cable, including a cable core, a cabling tape 5, an inner sheath 6, an armor layer 7, an armor outer protective tape 8 and an outer sheath 9 arranged in sequence from the inside to the outside. The outer sheath 9 is made of the above-mentioned cold-resistant sheath material. The cable core includes a plurality of twisted cores. Cabling filling materials 4 are provided between the cores and between the cores and the cabling tape 5. The core includes a conductor 1, a conductor wrapping tape 2 wrapped around the outside of the conductor 1, and an insulating layer 3 wrapped around the conductor wrapping tape 2. The invention can work normally at an ambient temperature of -60°C, thereby replacing ordinary shipboard cables that can only withstand low-temperature applications of -15°C, providing safe transmission guarantees for ships sailing in extremely cold areas, and ensuring safe use at extremely low ambient temperatures.

[0096] See also Figure 3 The present invention provides a method for manufacturing a cold-resistant shipboard cable, the manufacturing method comprising:

[0097] T1: Wire drawing and annealing process, the conductor raw material is drawn into a single wire of a set diameter. The conductor raw material will undergo work hardening during the drawing process. In order to restore the plasticity of the conductor raw material, the single wire is annealed and softened at high temperature. After the single wire is cooled in normal temperature water, it is blown dry with compressed air and wired onto the take-up reel;

[0098] T2: Bundling process, the drawn single wires are bundled into conductor units;

[0099] T3: re-twisting process, re-twisting the bundled conductor units into conductor 1 for the second time, and wrapping a layer of conductor wrapping tape 2 around the conductor 1;

[0100] T4: Insulation process, the insulating material is coated on the outside of the conductor wrapping tape 2, and the molecules of the insulating material are transformed from a linear structure to a mesh structure through steam cross-linking;

[0101] T5: Cabling process, filling the gap with cabling filling material 4, twisting the cable core into a round shape through a cabling and paralleling die, wrapping a layer of cabling wrapping tape 5 outside the cable core, and wrapping a layer of inner sheath 6 outside the cabling wrapping tape 5;

[0102] T6: Braided armor wrapping protection process, a specified number of braided wires are evenly woven outside the inner sheath 6 to form an armor layer 7, and an armor outer protection belt 8 is wrapped outside the armor layer 7;

[0103] T7: outer sheath process, using an extruder to first extrude and melt the above-mentioned cold-resistant sheath material, and then after being shaped by an extrusion die, it is coated on the outside of the armor outer protection belt 8 to form an outer sheath 9.

[0104] The present invention adopts thermosetting halogen-free low-smoke polyolefin material to replace the existing thermoplastic halogen-free low-smoke polyolefin material technology used in low-temperature environment, retains the mechanical and physical properties of thermoplastic materials, and solves the problem of relative conflict between the flame retardant performance and low-temperature resistance of thermosetting halogen-free low-smoke polyolefin materials; under the premise of meeting the low-temperature resistance, by adopting high flame retardant PP low-halogen filling rope and halogen-free low-smoke flame retardant glass fiber tape during cabling, the flame retardant performance and low halogen and low-smoke performance of the cable are improved from the cable structure and material; the flexibility of the cable is ensured by material selection and conductor process design and production process, so that the cable has an excellent bending radius; the physical, mechanical and shielding properties are excellent through the selection of armor materials and processes and process control; the low-temperature resistance and oil resistance are excellent through the selection of inner and outer sheath materials and the optimization of process structure.

[0105] The present invention provides an embodiment of a method for manufacturing a cold-resistant shipboard cable, the manufacturing method comprising:

[0106] T1: Wire drawing and annealing process: The conductor raw material is drawn into a single wire with a diameter of 0.25-0.4mm through a diamond wire drawing die with a gradually changing internal aperture. The single wire is annealed and softened in an oven at 500-600℃. The single wire is cooled in a 2-3m long water pipe at room temperature and then blown dry with compressed air and put on the take-up reel.

[0107] T2: Bundling process, the drawn single wires are bundled into a cross-sectional area of ​​1-16mm 2 The conductor unit adopts a high-speed double-twisted stranding machine. The single wires are twisted into bundles through the rotation of the twisting bow. The twisting pitch ratio is 8-10 times, and the twisting direction is left. At the same time, an active pay-off frame is used for pay-off. The tension of the pay-off and take-up wire is controlled to be constant. The tension is set between 10-15N to ensure that the DC resistance value of the manufactured cable conductor is stable and well controllable.

[0108] T3: Re-twisting process, the bundled conductor units are re-twisted to a cross-sectional area of ​​25-400mm 2 The conductor 1 is arranged in a regular stranded structure of 1+6+12+18, and the stranded pitch ratio is 10-12 times. Since the structure of Category 5 conductors is not stable enough, they will be flattened after being pulled. In order to prevent the round conductor from deforming, a layer of conductor wrapping tape 2 is wrapped around the conductor 1. The conductor wrapping tape 2 is a non-woven fabric with a nominal thickness of 0.16mm. The overlap rate exceeds 25%, and the wrapping direction is right-handed. The conductor is wound onto a reel through a traction wheel;

[0109] T4: Insulation process, a high-speed extruder is used to coat the insulating material on the outside of the conductor wrapping tape 2 in combination with the process requirements, and the molecules of the insulating material are converted from a linear structure to a mesh structure through steam cross-linking. The nominal thickness of the insulating layer 3 is 0.7-2.0 mm. Preferably, the insulating material is silane cross-linked polyethylene, and its tensile strength is greater than 13.5 MPa and its elongation is greater than 350%;

[0110] T5: Cabling process, fill the cabling filling material 4 into the gap, the cabling pitch-diameter ratio is 23-24 times, and the cable core is twisted into a circle through a cabling and paralleling die. Preferably, the cabling filling material 4 is a high flame retardant PP low-halogen filling rope, which requires an oxygen index greater than 26%, a pH value greater than 4.3, a conductivity less than 10μS / mm, HCl and HBr less than 0.5%, HF less than 0.1%, and a smoke density less than 100mg / m3. Wrap a layer of cabling wrapping tape 5 outside the cable core. The cabling wrapping tape 5 is a halogen-free, low-smoke, flame-retardant glass fiber tape, which requires an oxygen index greater than 55%, a pH value greater than 4.3, a conductivity less than 3μS / mm, and a smoke density less than 100mg / m 3 The nominal thickness of the cabling wrapping tape 5 is 0.17 mm, the overlap rate exceeds 25%, the wrapping direction is left, and a layer of inner sheath 6 is wrapped outside the cabling wrapping tape 5;

[0111] T6: Braided armor wrapping protection process, using a continuously variable speed braiding machine to evenly weave a specified number of braided wires on the outside of the inner sheath 6 to form an armor layer 7, the braiding density is required to be greater than 82%, and a layer of armor outer protection belt 8 is wrapped around the outside of the armor layer 7. The armor outer protection belt 8 is a non-woven dotted fabric with a nominal thickness of 0.1mm, an overlap rate of more than 25%, and the wrapping direction is left;

[0112] T7: outer sheath process, using an extruder to first extrude and melt the above-mentioned cold-resistant sheath material, and then after being shaped by an extrusion mold, it is coated on the outside of the armored outer protection belt 8 to form an outer sheath 9, the nominal thickness of the outer sheath 9 = cable core outer diameter × 0.025 + 0.6mm, the minimum nominal thickness is 0.8mm, preferably, the temperature of the extruder is: 90-110℃ in the feeding section, 140-160℃ in the melting section, 170-180℃ in the homogenizing section, 175-185℃ in the die head, and the screw compression ratio of the extruder is 1.8-2.

[0113] The comparison results of the temperature of each section of the extruder, the screw compression ratio and the existing materials are as follows:

[0114] Feeding section Melting section Homogenization section Die head Screw compression ratio Existing cables 130-140℃ 140-150℃ 150-160℃ 150-160℃ 1.2-1.6 Inventing the Cable 90-110℃ 140-160℃ 170-180℃ 175-185℃ 1.8-2

[0115] The cable material of the present invention uses ethylene-vinyl acetate copolymer and rubber material as base materials, the sheath material has a large shear force when being extruded, and the compression ratio of the extrusion screw is selected to be 1.8-2; the cable material of the present invention contains ethylene propylene diene monomer rubber, and the extrusion shear force is relatively large, so the temperature of the feeding section is lower than that of the existing cable, which is convenient for the material to be smoothly fed into the screw chamber. If the temperature is high, the rubber will melt and return material will occur; the cable material of the present invention contains ethylene propylene diene monomer rubber, and the extrusion temperature reaches 180°C, which is conducive to the full melting of the rubber material.

[0116] The test data of the cold-resistant shipboard cable of the present invention are as follows:

[0117]

[0118]

[0119] In summary, the present invention provides a cold-resistant sheath material and a preparation method, a cold-resistant shipboard cable and a manufacturing method, which have good tensile strength, elongation at break, oxygen index and oil resistance, and can work normally at an ambient temperature of -60°C, thereby replacing ordinary shipboard cables that can only withstand low-temperature application environments of -15°C, providing safe transmission guarantees for ships sailing in extremely cold areas, and ensuring safe use at extremely low ambient temperatures; using thermosetting halogen-free low-smoke polyolefin materials to replace the existing technology of using thermoplastic halogen-free low-smoke polyolefin materials in low-temperature environments, retaining the mechanical and physical properties of thermoplastic materials, and solving the problem of the relative conflict between the addition ratios of the two materials, namely, flame retardant properties and low-temperature resistance properties of thermosetting halogen-free low-smoke polyolefin materials; on the premise of meeting the low-temperature resistance performance, through cable forming High flame retardant PP low halogen filling rope and halogen-free low smoke flame retardant glass fiber tape are used to improve the flame retardant performance and low halogen and low smoke performance of the cable from the perspective of cable structure and materials; the flexibility of the cable is ensured by material selection and conductor process design and production process, so that the cable has an excellent bending radius; the physical, mechanical and shielding properties are excellent through the selection of armor materials and processes and process control; the low temperature resistance and oil resistance are excellent through the selection of inner and outer sheath materials and the optimization of process structure; the cable material contains EPDM rubber, and the extrusion shear force is large, so the temperature of the feeding section is lower than that of the existing cable, which is convenient for the material to be smoothly fed into the screw chamber. If the temperature is high, the rubber will melt and return material will occur; the cable material contains EPDM rubber, and the extrusion temperature reaches 180℃, which is conducive to the full melting of the rubber material.

[0120] It should be emphasized that the above are only preferred embodiments of the present invention and do not limit the present invention in any form. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A cold-resistant sheath material, characterized in that: Made from the following raw materials in parts by weight:

2. The cold-resistant sheath material according to claim 1, characterized in that: The flame retardant is aluminum hydroxide, and the compatibilizer is maleic anhydride grafted ethylene vinyl acetate.

3. A method for preparing a cold-resistant sheath material as claimed in claim 1 or 2, characterized in that: The preparation method comprises: S1: Mix polyolefin powder and modifier evenly according to proportion; S2: adding flame retardant to the mixture and adding it to a high-speed mixer for high-speed stirring; S3: adding ethylene-vinyl acetate copolymer, ethylene propylene diene monomer rubber, compatibilizer, antioxidant, lubricant and cross-linking agent into the mixture according to the formula ratio, and placing the mixture into a high-speed mixer for low-speed stirring; S4: putting the mixture into a twin-screw extruder for extrusion granulation and drying.

4. The preparation method according to claim 3, characterized in that: In step S2, the high-speed stirring temperature is 40-45°C.

5. The preparation method according to claim 3, characterized in that: In step S3, the low-speed stirring time is 4-6 minutes.

6. The preparation method according to claim 3, characterized in that: In step S4, the extrusion temperature of the granulation is 180°C and the drying temperature is 85°C.

7. A cold-resistant shipboard cable, characterized in that: The invention comprises a cable core, a cabling wrapping tape (5), an inner sheath (6), an armor layer (7), an armor outer protection tape (8) and an outer sheath (9) which are arranged in sequence from the inside to the outside. The outer sheath (9) is made of the cold-resistant sheath material as claimed in claim 1 or 2. The cable core comprises a plurality of twisted cores. Cabling filling materials (4) are provided between the cores and between the cores and the cabling wrapping tape (5). The core comprises a conductor (1), a conductor wrapping tape (2) wrapped around the outside of the conductor (1), and an insulating layer (3) wrapped around the conductor wrapping tape (2).

8. A method for manufacturing a cold-resistant shipboard cable as claimed in claim 7, characterized in that: The production method comprises: T1: Wire drawing and annealing process, the conductor raw material is drawn into a single wire of a set diameter, the single wire is annealed and softened at high temperature, the single wire is cooled in normal temperature water, and then blown dry with compressed air and wired onto the take-up reel; T2: Bundling process, the drawn single wires are bundled into conductor units; T3: a re-twisting process, in which the bundled conductor units are re-twisted into a conductor (1), and a layer of conductor wrapping tape (2) is wrapped around the conductor (1); T4: Insulation process, coating the insulating material on the outside of the conductor wrapping tape (2), and converting the molecules of the insulating material from a linear structure to a mesh structure through steam cross-linking; T5: Cabling process, filling the gap with a cabling filling material (4), twisting the cable core into a round shape through a cabling and paralleling die, wrapping a layer of cabling wrapping tape (5) around the cable core, and wrapping a layer of inner sheath (6) around the cabling wrapping tape (5); T6: braided armor wrapping protection step, uniformly weaving a specified number of braided wires on the outside of the inner sheath (6) to form an armor layer (7), and wrapping an armor outer protection belt (8) on the outside of the armor layer (7); T7: outer sheath process, using an extruder to first extrude and melt the cold-resistant sheath material as claimed in claim 1 or 2, and then after being shaped by an extrusion die, it is coated on the outside of the armor outer protection belt (8) to form an outer sheath (9).

9. The manufacturing method according to claim 8, characterized in that: The temperatures of the extruder are: 90-110°C in the feeding section, 140-160°C in the melting section, 170-180°C in the homogenizing section, and 175-185°C in the die head. The screw compression ratio of the extruder is 1.8-2.

10. The manufacturing method according to claim 8, characterized in that: The diameter of the single wire is 0.25-0.4 mm, the annealing temperature is 500-600° C., and the cross-sectional area of ​​the conductor unit is 1-16 mm. 2 The cross-sectional area of ​​the conductor (1) is 25-400 mm 2 .

11. The manufacturing method according to claim 8, characterized in that: The conductor wrapping tape (2) is a non-woven fabric, the nominal thickness of the conductor wrapping tape (2) is 0.16 mm, the overlap rate exceeds 25%, and the wrapping direction is right; the cabling wrapping tape (5) is a halogen-free low-smoke flame-retardant glass fiber tape, the nominal thickness of the cabling wrapping tape (5) is 0.17 mm, the overlap rate exceeds 25%, and the wrapping direction is left; the armor outer protection tape (8) is a non-woven dotted fabric, the nominal thickness of the armor outer protection tape (8) is 0.1 mm, the overlap rate exceeds 25%, and the wrapping direction is left.

12. The manufacturing method according to claim 8, characterized in that: The insulating material is silane cross-linked polyethylene, and the cable filling material (4) is a highly flame-retardant PP low-halogen filling rope.

Citation Information

Cited By

  • Cold-resistant sheath material and preparation method therefor, and cold-resistant marine cable and manufacturing method therefor