A medium-carbon chromium-nickel-molybdenum alloy structural steel and its surface quality control method

By combining titanium microalloying and nitrogen-controlled smelting processes with low-temperature heating rolling, the problem of poor surface quality caused by the coarse microstructure of continuous casting billets of medium-carbon chromium-nickel-molybdenum alloy structural steel was solved, resulting in a significant reduction in steel surface defects and a high surface qualification rate.

CN118703868BActive Publication Date: 2026-11-17DAYE SPECIAL STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410861956.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2026-11-17
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

The coarse microstructure of continuously cast billets of medium carbon chromium-nickel-molybdenum alloy structural steel (100mm < ∮ ≤ 160mm) results in poor surface quality, making them prone to longitudinal cracks and overheating coarse grains, which affects the surface quality of the steel.

Method used

The process employs titanium microalloying and controlled aluminum and nitrogen smelting techniques, combined with low-temperature heating rolling technology, to control the titanium content to 0.0080-0.0120% and the heating temperature to 1220-1240℃. This precise control of the heating temperature range prevents the steel from developing coarse grains.

Benefits of technology

It effectively reduces surface defects in continuously cast billets, ensures that the surface quality of steel is within 0.3mm, improves the surface qualification rate of steel to more than 90%, and solves the problem of poor surface quality caused by coarse microstructure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118703868B_ABST
    Figure CN118703868B_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of medium-carbon chromium-nickel-molybdenum alloy structural steel preparation, and particularly relates to a medium-carbon chromium-nickel-molybdenum alloy structural steel and its surface quality control method. The method includes: sequentially smelting, continuously casting, and rolling the raw material of the medium-carbon chromium-nickel-molybdenum alloy structural steel to obtain the steel; wherein, during smelting, titanium microalloying treatment and aluminum and nitrogen control are performed, controlling the titanium content to 0.0080-0.0120%; the rolling process includes low-temperature heating rolling, with the low-temperature heating temperature being 1220-1240℃. Due to the titanium microalloying treatment and aluminum and nitrogen control during smelting, and the low-temperature heating rolling, the continuously cast billet has a fine microstructure and significantly reduced surface defects, avoiding the generation of large-size defect depths. This solves the problem of poor surface quality caused by the coarse microstructure of large-size quenched and tempered 39NiCrMo3 round steel, ensuring that the surface defect depth of the steel is within 0.3mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of medium carbon chromium-nickel-molybdenum alloy structural steel preparation, and in particular relates to a medium carbon chromium-nickel-molybdenum alloy structural steel and its surface quality control method. Background Technology

[0002] Medium-carbon chromium-nickel-molybdenum alloy structural steel 39CrNiMo3 requires good surface quality, with the depth of black-skinned surface defects not exceeding 0.3mm.

[0003] However, for 39NiCrMo3 quenched and tempered round steel with specifications (100mm < ∮ ≤ 160mm), due to the thin shell of the continuously cast billet and the use of traditional smelting methods, the structure of the continuously cast billet is coarse, with well-developed columnar crystals and large differences between the inner and outer arc surfaces. Longitudinal cracks of varying depths are easily found on the surface of the billet, resulting in poor surface quality of the steel.

[0004] For 39NiCrMo3 quenched and tempered round steel with specifications (100mm < ∮ ≤ 160mm), due to the large size of the continuously cast billet, the traditional heating method is used, and the heating temperature is high. The steel surface is easily overheated, resulting in coarse grains. At the same time, the high Al and N content makes it easy for them to precipitate at the grain boundaries. The cumulative effect leads to cracking.

[0005] In view of this, the present invention is hereby proposed. Summary of the Invention

[0006] To address the shortcomings and defects of existing technologies, the present invention aims to provide a medium-carbon chromium-nickel-molybdenum alloy structural steel and a method for controlling its surface quality. The method employs titanium microalloying treatment and controlled aluminum and nitrogen during smelting, resulting in a fine microstructure and significantly reduced surface defects in the continuously cast billet, avoiding the formation of large-sized defects and ensuring that surface defects are within 0.3 mm. Furthermore, by adopting a new heating rolling process and precisely controlling the heating temperature range of 1220℃ to 1240℃, the steel is fully heated through, achieving fine grains while remaining within the high-temperature plastic deformation range, thus keeping the surface defect depth within 0.3 mm. This solves the problem of poor surface quality caused by the coarse microstructure of large-diameter quenched and tempered 39NiCrMo3 round steel.

[0007] To achieve the above objectives, the present invention adopts the following technical solution:

[0008] In a first aspect, a method for surface quality control of medium-carbon chromium-nickel-molybdenum alloy structural steel includes: sequentially smelting, continuously casting, and rolling the raw material of the medium-carbon chromium-nickel-molybdenum alloy structural steel to obtain the medium-carbon chromium-nickel-molybdenum alloy structural steel; wherein, during the smelting process, titanium microalloying treatment and aluminum and nitrogen control are performed, and the titanium content is controlled to be 0.0080-0.0120%; the rolling process includes low-temperature heating rolling, and the low-temperature heating temperature is 1220-1240℃.

[0009] Furthermore, during the smelting process, vacuum degassing is employed with a vacuum degree ≤0.5 Torr and a total vacuum time of 20-35 minutes. Simultaneously, argon soft blowing is used for 20-35 minutes to control aluminum and nitrogen levels.

[0010] Furthermore, the aluminum control refers to controlling the aluminum content to 0.010%-0.025%; the nitrogen control refers to controlling the nitrogen content to be less than or equal to 0.0070%.

[0011] Furthermore, the primary refining adopts converter primary refining, which involves adding scrap steel and molten iron, and then melting, dephosphorizing, decarburizing and alloying in a converter under an oxidizing atmosphere. The carbon content at the end of the converter is ≥0.08%, the phosphorus content is controlled to be ≤0.015%, and the tapping temperature is 1620-1650℃.

[0012] And / or, after ladle refining, the sulfur content is controlled to be ≤0.005%, the titanium content is controlled to be 0.008-0.012%, and the tapping temperature is 1595-1635℃.

[0013] Furthermore, the billet obtained by continuous casting is a square billet with dimensions of 410*530mm.

[0014] Furthermore, the continuous casting temperature is 1515-1530℃, and the casting speed is 0.41-0.45m / min;

[0015] And / or, the rolling process includes final rolling, wherein the temperature of the final rolling is not lower than 860°C.

[0016] Furthermore, the medium-carbon chromium-nickel-molybdenum alloy structural steel obtained by rolling is a round bar with a specification of 100mm < ∮ ≤ 160mm.

[0017] Secondly, a medium-carbon chromium-nickel-molybdenum alloy structural steel is prepared by the aforementioned surface quality control method.

[0018] Furthermore, the medium-carbon chromium-nickel-molybdenum alloy structural steel is made of 39NiCrMo3.

[0019] Furthermore, the chemical composition of the 39NiCrMo3, by mass percentage, is as follows: C 0.35-0.43%, Si 0.15-0.40%, Mn 0.50-0.80%, P≤0.025%, S≤0.035%, Cr 0.60-1.00%, Ni 0.70-1.00%, Mo 0.15-0.25%, V≤0.05%, Cu≤0.30%, Ti 0.0080-0.0120%, Al 0.010-0.025%, N≤0.0070%, with the balance being Fe and unavoidable impurities.

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0021] This invention discloses a surface quality control method for carbon-chromium-nickel-molybdenum alloy structural steel. By employing a novel smelting method and a smelting process involving micro-titanium alloying and controlled aluminum and nitrogen, the surface quality of continuously cast billets is effectively improved. Simultaneously, the use of low-temperature heating and rolling avoids grain growth in the steel, reducing the likelihood of surface quality deterioration due to excessively high heating temperatures. The solidification structure of the continuously cast billet, from the outside in, consists of: a chilled layer (fine equiaxed crystals), a columnar crystal region, and a central equiaxed crystal region. The finer the internal crystals, the less prone the surface is to crack defects. Therefore, the use of titanium micro-alloying and controlled aluminum and nitrogen effectively controls the morphology and size of the continuously cast billet's microstructure, significantly reducing surface defects and preventing the formation of large-scale defects. Furthermore, the use of a novel heating rolling process, precisely controlling the heating temperature range of 1220℃ to 1240℃, ensures the steel is fully heated through, maintaining fine grains within the high-temperature plastic deformation range. This prevents the billet from remaining in the high-temperature range for extended periods, which can lead to coarse grains and negatively impact surface quality.

[0022] The method of this invention can solve the problem of poor surface quality of large-size quenched and tempered 39NiCrMo3 round steel due to coarse microstructure. It is applicable to the preparation of quenched and tempered 39NiCrMo3 round steel with specifications (100mm < ∮ ≤ 160mm). The surface defect depth of the prepared steel is within 0.3mm, and the surface qualification rate of the steel is greatly improved to no less than 90%. Attached Figure Description

[0023] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0024] Figure 1 This is a flowchart of the method of the present invention;

[0025] Figure 2 This is a 500x metallographic photograph of the 1 / 2 radius portion of the 39NiCrMo3 round steel bar obtained in Example 1 of the present invention;

[0026] Figure 3 This is a 100x metallographic photograph of the 1 / 2 radius portion of the 39NiCrMo3 round steel bar obtained in Example 1 of the present invention;

[0027] Figure 4This is a 100x metallographic photograph of the 1 / 2 radius portion of the 39NiCrMo3 round steel bar obtained in Comparative Example 4 of this invention. Detailed Implementation

[0028] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Those skilled in the art should understand that the embodiments described are merely illustrative of the invention and should not be considered as specific limitations thereof. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention. Process parameters not specifically specified in the following embodiments are generally performed under conventional conditions.

[0029] The endpoints and any values ​​of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.

[0030] According to a first aspect of the present invention, a method for surface quality control of medium-carbon chromium-nickel-molybdenum alloy structural steel is provided, wherein the raw material of the medium-carbon chromium-nickel-molybdenum alloy structural steel is sequentially smelted, continuously cast, and rolled to obtain the medium-carbon chromium-nickel-molybdenum alloy structural steel; wherein, during the smelting process, titanium microalloying treatment and aluminum and nitrogen control are performed, and the titanium content is controlled to be 0.0080-0.0120%; the rolling process includes low-temperature heating rolling, wherein the low-temperature heating temperature is 1220-1240℃.

[0031] This invention pioneers a surface quality control method for medium-carbon chromium-nickel-molybdenum alloy structural steel. Employing micro-titanium alloying and controlled aluminum and nitrogen smelting processes, it effectively improves the surface quality of continuously cast billets. Simultaneously, by using low-temperature heating and rolling, it avoids grain growth in the steel, reducing the probability of surface quality deterioration caused by excessively high heating temperatures. This solves the problem of poor surface quality in large-diameter quenched and tempered 39NiCrMo3 round steel due to its coarse microstructure. Specifically, 1. By adopting a new smelting method and titanium micro-alloying treatment, the titanium content is controlled at 0.0080-0.0120% (e.g., 0.0085%, 0.0090%, 0.0095%, 0.0100%, 0.0105%, 0.0115%, etc.), and the aluminum and nitrogen content is kept low, so that the surface defect depth of the continuously cast billet is within 0.3mm, meeting surface requirements. 2. 39NiCrMo3 continuously cast square billets with specifications of 410*530mm are rolled in a walking beam furnace at a heating temperature of 1220℃~1240℃ (such as 1221℃, 1223℃, 1225℃, 1227℃, 1229℃, 1231℃, 1233℃, 1235℃, 1237℃, 1239℃, etc.) to avoid prolonged residence of the billet in the high-temperature section, which would cause coarse grains and be detrimental to surface quality. This process yields a balanced structure of pearlite and ferrite, meeting the surface requirements.

[0032] In this invention, titanium is microalloyed during the refining process by adding titanium-iron alloy according to the target composition. The titanium content is controlled at 0.0080-0.0120%. If the titanium content is too high, it will affect the quality of the steel, especially its impact performance; if the titanium content is too low, the surface quality improvement effect will be poor.

[0033] As an optional embodiment of the surface quality control method of the present invention, during the smelting process, vacuum degassing is adopted, with a vacuum degree ≤0.5 Torr (e.g., 0.4 Torr, 0.3 Torr, 0.2 Torr, 0.1 Torr, etc.), and a total vacuum time of 20-35 min (e.g., 21 min, 23 min, 25 min, 27 min, 29 min, 31 min, 33 min, etc.). At the same time, argon gas soft blowing is adopted, with a soft blowing time of 20-35 min (e.g., 21 min, 23 min, 25 min, 27 min, 29 min, 31 min, 33 min, etc.), to control aluminum and nitrogen. Further, the aluminum control refers to controlling the aluminum content to 0.010%-0.025% (e.g., 0.011%, 0.013%, 0.015%, 0.017%, 0.019%, 0.021%, 0.023%, etc.); the nitrogen control refers to controlling the nitrogen content to be less than or equal to 0.0070% (e.g., 0.0070%, 0.0065%, 0.0060%, 0.0055%, 0.0050%, 0.0045%, 0.0040%, 0.0035%, etc.). Excessive aluminum and nitrogen content can easily lead to surface cracks precipitating at grain boundaries, while insufficient aluminum content results in coarse grains and reduced impact strength.

[0034] The present invention further provides a method for surface quality control of the above-mentioned medium carbon chromium nickel molybdenum steel, comprising the following steps:

[0035] (a) Smelting: The raw materials are smelted through primary smelting, ladle refining, and vacuum degassing to obtain molten steel;

[0036] (b) Casting: The molten steel is continuously cast to obtain a continuously cast billet;

[0037] (c) Rolling: The continuous casting billet is shaped into round steel.

[0038] Based on the above-described technical solution of this invention, in step (a), a converter primary refining process is adopted. This involves adding scrap steel and molten iron, followed by melting, dephosphorization, decarburization, and alloying in a converter under an oxidizing atmosphere. The final carbon content at the converter endpoint is ≥0.08% (e.g., 0.08%, 0.085%, 0.09%, 0.095%, 0.1%, 0.105%, 0.115%, etc.), and the phosphorus content is controlled to ≤0.015% (e.g., 0.015%, 0.012%, 0.010%, 0.008%, 0.005%, 0.003%, 0.0...). The steelmaking temperature is 1620-1650℃ (e.g., 1625℃, 1630℃, 1635℃, 1640℃, 1645℃, etc.); after ladle refining, the sulfur content is controlled to ≤0.005% (e.g., 0.005%, 0.004%, 0.003%, 0.002%, 0.001%, etc.), and the titanium content is controlled to 0.008-0.012% (e.g., 0.0085%, 0.0090%, 0.0095%, 0.0100%, 0.0105%, 0.0115%, etc.), and the steelmaking temperature is... 1595-1635℃ (e.g., 1600℃, 1605℃, 1610℃, 1615℃, 1620℃, 1625℃, 1630℃, etc.); vacuum degassing, vacuum degree ≤0.5 Torr (e.g., 0.4 Torr, 0.3 Torr, 0.2 Torr, 0.1 Torr, etc.), total vacuum time 20-35 min (e.g., 21 min, 23 min, 25 min, 27 min, 29 min, 31 min, 33 min, etc.), simultaneously using argon soft blowing, soft blowing time 20-35 min (e.g., 21 min, 23 min, 2... 5 min, 27 min, 29 min, 31 min, 33 min, etc.), control the aluminum content to 0.010-0.025% (e.g., 0.011%, 0.013%, 0.015%, 0.017%, 0.019%, 0.021%, 0.023%, etc.), and control the nitrogen content to be less than or equal to 0.0070% (e.g., 0.0070%, 0.0065%, 0.0060%, 0.0055%, 0.0050%, 0.0045%, 0.0040%, 0.0035%, etc.).

[0039] Based on the above-mentioned technical solution of the present invention, in step (b), induction heating of a steel ladle is used to pour molten steel into the tundish at a certain speed. The molten steel passes through a water-cooled crystallizer, where it solidifies into a hard shell and is continuously pulled out from the bottom outlet of the crystallizer. After being cooled by water spray, it is completely solidified. The liquidus of 39NiCrMo3 is 1495℃, the continuous casting temperature is 1515-1530℃ (such as 1516℃, 1518℃, 1520℃, 1522℃, 1524℃, 1526℃, 1528℃, etc.), the continuous casting billet is 410*530mm, and the casting speed is 0.41~0.45m / min (such as 0.42m / min, 0.43m / min, 0.44m / min, etc.).

[0040] Based on the above-described technical solution of this invention, in step (c), the continuously cast billet is heated to 1220-1240℃ (e.g., 1221℃, 1223℃, 1225℃, 1227℃, 1229℃, 1231℃, 1233℃, 1235℃, 1237℃, 1239℃, etc.) and fully heated. Then, it is rolled using a 1350 mill and finished using a 750 mill, resulting in a round bar shape. The final rolling temperature is not lower than 860℃ (e.g., 860℃, 865℃, 870℃, 875℃, 880℃, 885℃, 890℃, 895℃, 900℃, etc.). Further, the round bar specifications are 100mm < ∮ ≤ 160mm (e.g., ∮110mm, ∮120mm, ∮130mm, ∮140mm, ∮150mm, etc.).

[0041] According to a second aspect of the present invention, a medium-carbon chromium-nickel-molybdenum alloy structural steel is prepared by the surface quality control method described above.

[0042] As an optional embodiment of the carbon-chromium-nickel-molybdenum alloy structural steel of the present invention, the material of the carbon-chromium-nickel-molybdenum alloy structural steel is 39NiCrMo3. More specifically, the 39NiCrMo3, by mass percentage, has the following chemical composition: C 0.35-0.43%, Si 0.15-0.40%, Mn 0.50-0.80%, P≤0.025%, S≤0.035%, Cr 0.60-1.00%, Ni 0.70-1.00%, Mo 0.15-0.25%, V≤0.05%, Cu≤0.30%, Ti 0.0080-0.0120%, Al 0.010-0.025%, N≤0.0070%, with the balance being Fe and unavoidable impurities.

[0043] The present invention will now be described in further detail with reference to specific embodiments and comparative examples.

[0044] Example 1

[0045] A method for surface quality control of medium-carbon chromium-nickel-molybdenum alloy structural steel includes the following steps:

[0046] (a) Smelting: The raw materials are smelted through primary smelting, ladle refining, and vacuum degassing to obtain molten steel;

[0047] (d) Casting: The molten steel is continuously cast to obtain a continuously cast billet;

[0048] (e) Rolling: The continuous casting billet is shaped into round steel.

[0049] In step (a), a converter primary refining process is adopted, in which scrap steel and molten iron are added, and then melting, dephosphorization, decarburization and alloying are carried out in a converter under an oxidizing atmosphere. The carbon content at the end of the converter is 0.012%, the phosphorus content is controlled at 0.013%, and the tapping temperature is 1630℃. After ladle refining, the sulfur content is controlled at 0.002%, the titanium content is controlled at 0.0092%, and the tapping temperature is 1605℃. Vacuum degassing is performed with a vacuum degree ≤0.5 Torr and a total vacuum time of 25 min. At the same time, argon soft blowing is used for 30 min, and the aluminum content is controlled at 0.017% and the nitrogen content is controlled at 0.0041%.

[0050] In step (b), induction heating is used to pour molten steel into the tundish at a certain speed. The molten steel passes through a water-cooled crystallizer, where it solidifies into a hard shell and is continuously pulled out from the bottom outlet of the crystallizer. After being cooled by water spray, it is completely solidified. The liquidus of 39NiCrMo3 is 1495℃, the continuous casting temperature is 1520℃, the continuous casting billet is 410*530mm, and the casting speed is 0.43m / min.

[0051] In step (c), the continuously cast billet is heated to 1230°C and fully heated. Then, it is rolled on a 1350 mill and finished on a 750 mill, with the final shape being round steel and the final rolling temperature being 880°C.

[0052] The 39NiCrMo3 round steel bar obtained in Example 1 has a diameter of ∮130mm and includes the following chemical composition by mass fraction: C 0.40%, Si 0.25%, Mn 0.75%, P 0.013%, S 0.002%, Cr 0.92%, Ni 0.76%, Mo 0.18%, V 0.008%, Cu 0.02%, Ti 0.0098%, Al 0.017%, N 0.0041%, with the balance being Fe and unavoidable impurities.

[0053] Example 2

[0054] A method for surface quality control of medium-carbon chromium-nickel-molybdenum alloy structural steel includes the following steps:

[0055] (a) Smelting: The raw materials are smelted through primary smelting, ladle refining, and vacuum degassing to obtain molten steel;

[0056] (f) Casting: The molten steel is continuously cast to obtain a continuously cast billet;

[0057] (g) Rolling: The continuous casting billet is shaped into round steel.

[0058] In step (a), a converter primary refining process is adopted, in which scrap steel and molten iron are added, and then melting, dephosphorization, decarburization and alloying are carried out in a converter under an oxidizing atmosphere. The carbon content at the end of the converter is 0.08%, the phosphorus content is controlled at 0.015%, and the tapping temperature is 1650℃. After ladle refining, the sulfur content is controlled at 0.005%, the titanium content is controlled at 0.012%, and the tapping temperature is 1635℃. Vacuum degassing is performed with a vacuum degree ≤0.5 Torr and a total vacuum time of 20 min. At the same time, argon soft blowing is used for 20 min, and the aluminum content is controlled at 0.025% and the nitrogen content is controlled at 0.0070%.

[0059] In step (b), induction heating is used to pour molten steel into the tundish at a certain speed. The molten steel passes through a water-cooled crystallizer, where it solidifies into a hard shell and is continuously pulled out from the bottom outlet of the crystallizer. After being cooled by water spray, it is completely solidified. The liquidus of 39NiCrMo3 is 1495℃, the continuous casting temperature is 1530℃, the continuous casting billet is 410*530mm, and the casting speed is 0.45m / min.

[0060] In step (c), the continuously cast billet is heated to 1240°C and fully heated. Then, it is rolled on a 1350 mill and finished on a 750 mill, with the final shape being round steel and the final rolling temperature being 890°C.

[0061] The obtained 39NiCrMo3 round steel bar has a diameter of ∮160mm and includes the following chemical composition by mass fraction: C 0.43%, Si 0.40%, Mn 0.80%, P 0.025%, S 0.035%, Cr 1.00%, Ni 1.00%, Mo 0.25%, V 0.05%, Cu 0.30%, Ti 0.0120%, Al 0.025%, N 0.0070%, with the balance being Fe and unavoidable impurities.

[0062] Example 3

[0063] A method for surface quality control of medium-carbon chromium-nickel-molybdenum alloy structural steel includes the following steps:

[0064] (a) Smelting: The raw materials are smelted through primary smelting, ladle refining, and vacuum degassing to obtain molten steel;

[0065] (h) Casting: The molten steel is continuously cast to obtain a continuously cast billet;

[0066] (i) Rolling: The continuous casting billet is shaped into round steel.

[0067] In step (a), a converter primary refining process is adopted, in which scrap steel and molten iron are added, and then melting, dephosphorization, decarburization and alloying are carried out in a converter under an oxidizing atmosphere. The carbon content at the converter endpoint is 0.011%, the phosphorus content is controlled at 0.012%, and the tapping temperature is 1620℃. After ladle refining, the sulfur content is controlled at 0.003%, the titanium content is controlled at 0.008%, and the tapping temperature is 1595℃. Vacuum degassing is performed with a vacuum degree ≤0.5 Torr and a total vacuum time of 35 min. At the same time, argon soft blowing is used for 35 min, and the aluminum content is controlled at 0.010% and the nitrogen content is controlled at 0.0030%.

[0068] In step (b), induction heating is used to pour molten steel into the tundish at a certain speed. The molten steel passes through a water-cooled crystallizer, where it solidifies into a hard shell and is continuously pulled out from the bottom outlet of the crystallizer. After being cooled by water spray, it is completely solidified. The liquidus of 39NiCrMo3 is 1495℃, the continuous casting temperature is 1515℃, the continuous casting billet is 410*530mm, and the casting speed is 0.41m / min.

[0069] In step (c), the continuously cast billet is heated to 1220°C and fully heated. Then, it is rolled on a 1350 mill and finished on a 750 mill, with the final shape being round steel and the final rolling temperature being 860°C.

[0070] The obtained 39NiCrMo3 round steel bar has a diameter of ∮100mm and includes the following chemical composition by mass fraction: C 0.35%, Si 0.15%, Mn 0.50%, P 0.012%, S 0.003%, Cr 0.60%, Ni 0.70%, Mo 0.15%, V 0.015%, Cu 0.08%, Ti 0.0080%, Al 0.010%, N 0.0030%, with the balance being Fe and unavoidable impurities.

[0071] Comparative Example 1

[0072] This comparative example provides a surface control method for medium-carbon chromium-nickel-molybdenum alloy structural steel. Except for adjusting the Ti composition to 0.0030% during smelting, the other steps are the same as in Example 1.

[0073] The 39NiCrMo3 round steel obtained in Comparative Example 1 has the following chemical composition by mass fraction: C 0.40%, Si 0.26%, Mn 0.74%, P 0.014%, S 0.003%, Cr 0.91%, Ni 0.75%, Mo 0.18%, V 0.007%, Cu 0.02%, Ti 0.0030%, Al 0.017%, N 0.0041%, with the balance being Fe and unavoidable impurities.

[0074] Comparative Example 2

[0075] This comparative example provides a surface control method for medium-carbon chromium-nickel-molybdenum alloy structural steel. Except for adjusting the Al content to 0.03% during smelting, the other steps are the same as in Example 1.

[0076] The resulting 39NiCrMo3 round steel has the following chemical composition by mass fraction: C 0.40%, Si 0.25%, Mn 0.75%, P 0.013%, S 0.002%, Cr 0.92%, Ni 0.76%, Mo 0.18%, V 0.008%, Cu 0.02%, Ti 0.0098%, Al 0.03%, N 0.0041%, with the balance being Fe and unavoidable impurities.

[0077] Comparative Example 3

[0078] This comparative example provides a surface control method for medium-carbon chromium-nickel-molybdenum alloy structural steel. Except for adjusting the N composition to 0.0080% during smelting, the other steps are the same as in Example 1.

[0079] The resulting 39NiCrMo3 round steel has the following chemical composition by mass fraction: C 0.40%, Si 0.25%, Mn 0.75%, P 0.013%, S 0.002%, Cr 0.92%, Ni 0.76%, Mo 0.18%, V 0.008%, Cu 0.02%, Ti 0.0098%, Al 0.0017%, N 0.0080%, with the balance being Fe and unavoidable impurities.

[0080] Comparative Example 4

[0081] This comparative example provides a surface control method for medium carbon chromium nickel molybdenum alloy structural steel. Except for adjusting the rolling temperature to 1250°C, the other steps are the same as in Example 1.

[0082] test

[0083] Magnetic particle testing was performed on the 39NiCrMo3 bars obtained in the examples and comparative examples using a CDW-24000AT instrument. The specific test results are as follows:

[0084] project Number of surface defects on a single piece Percentage of surface defects Example 1 1-5 5% Example 2 1-5 10% Example 3 1-5 7% Comparative Example 1 5-30 places 90% Comparative Example 2 1-5 15% Comparative Example 3 5-15 35% Comparative Example 4 5-15 30%

[0085] Note: Defects with a depth of 0.3 mm or more are considered unqualified defects. Bars with unqualified defects on their surface are considered surface unqualified bars. The surface unqualified percentage rate for each embodiment and comparative example is the number of unqualified bars / the total number of tested bars × 100%. For example, the surface unqualified percentage rate of Example 1 = the number of unqualified bars in Example 1 / the total number of tested bars in Example 1 × 100%.

[0086] At the same time, through Figure 2 , 3 It can be seen from the metallographic structure of the 39NiCrMo3 round steel bar at half its radius obtained in Example 1 that the controlled method of this invention yielded a balanced microstructure of pearlite and ferrite, and... Figure 4 Compared to bars obtained by medium- and high-temperature rolling, the control method of this invention greatly refines the grain size.

[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for surface quality control of medium-carbon chromium-nickel-molybdenum alloy structural steel, characterized in that, include: The raw materials for the medium-carbon chromium-nickel-molybdenum alloy structural steel are sequentially smelted, continuously cast, and rolled to obtain the medium-carbon chromium-nickel-molybdenum alloy structural steel; wherein, during the smelting process, titanium microalloying treatment and controlled aluminum and nitrogen content are performed, with the titanium content controlled at 0.0080-0.0120%; the aluminum content is controlled at 0.010%-0.025%; and the nitrogen content is controlled at less than or equal to 0.0070%. The rolling forming includes low-temperature heating rolling, wherein the low-temperature heating temperature is 1220-1240℃; The medium-carbon chromium-nickel-molybdenum alloy structural steel obtained by rolling is a round bar with a specification of 100mm < ∮ ≤ 160mm and the surface defect depth of the steel is within 0.3mm; The medium-carbon chromium-nickel-molybdenum alloy structural steel is made of 39NiCrMo3. The chemical composition of 39NiCrMo3, by mass percentage, is: C 0.35-0.43%, Si 0.15-0.40%, Mn 0.50-0.80%, P≤0.025%, S≤0.035%, Cr0.60-1.00%, Ni 0.70-1.00%, Mo 0.15-0.25%, V≤0.05%, Cu≤0.30%, Ti 0.0080-0.0120%, Al 0.010-0.025%, N≤0.0070%, with the balance being Fe and unavoidable impurities.

2. The surface quality control method as described in claim 1, characterized in that, During the smelting process, vacuum degassing is employed with a vacuum degree ≤0.5 Torr and a total vacuum time of 20-35 minutes. Simultaneously, argon gas is used for soft blowing for 20-35 minutes to control aluminum and nitrogen levels.

3. The surface quality control method as described in claim 1, characterized in that, The smelting process includes primary smelting and ladle refining.

4. The surface quality control method as described in claim 3, characterized in that, The primary refining process is carried out in a converter. By adding scrap steel and molten iron, the steel is melted, dephosphorized, decarburized and alloyed in a converter under an oxidizing atmosphere. The carbon content at the end of the converter is ≥0.08%, the phosphorus content is controlled to be ≤0.015%, and the tapping temperature is 1620-1650℃. And / or, after ladle refining, the sulfur content is controlled to be ≤0.005%, the titanium content is controlled to be 0.008-0.012%, and the tapping temperature is 1595-1635℃.

5. The surface quality control method as described in claim 1, characterized in that, The billet obtained by continuous casting is a square billet with a specification of 410. 530mm.

6. The surface quality control method as described in claim 1, characterized in that, The continuous casting temperature is 1515-1530℃, and the casting speed is 0.41~0.45m / min; And / or, the rolling process includes final rolling, wherein the temperature of the final rolling is not lower than 860°C.

7. A medium-carbon chromium-nickel-molybdenum alloy structural steel, characterized in that, Prepared by the surface quality control method according to any one of claims 1-6.

Citation Information

Patent Citations

  • Ultrahigh tough steel plate with low yield ratio and preparation method thereof

    CN103060715A