Hydrogel dressing for diabetic wound repair and preparation method thereof

By using hydrogel dressings of polyvinyl alcohol, flavonoid small molecules and antioxidant polymers in diabetic wound repair, the problems of insufficient antioxidant capacity and poor polarization capacity of regenerative macrophages in the existing technology are solved. More effective diabetic wound healing and immune regulation achieved.

CN118718077APending Publication Date: 2024-10-01PEKING UNIV SCHOOL OF STOMATOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410750920.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Hydrogel dressings used for diabetic wound repair in the prior art have limited antioxidant capacity and cannot effectively regulate regenerative macrophage polarization, resulting in difficulty in diabetic wound healing.

Method used

A hydrogel dressing containing polyvinyl alcohol, flavonoid small molecules and an antioxidant polymer is used. The antioxidant polymer contains a boronic acid group and a dihydropyrimidinone structure. The flavonoid small molecules are grafted on the antioxidant polymer. Enhances antioxidant properties and modulates immune response.

Benefits of technology

It significantly enhances the antioxidant capacity and immune regulation ability of the hydrogel, promotes diabetic wound healing, and provides better industrial production conditions and a simple preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718077A_ABST
    Figure CN118718077A_ABST
Patent Text Reader

Abstract

The invention provides a hydrogel dressing for diabetic wound repair. The hydrogel dressing comprises polyvinyl alcohol, flavonoid micromolecules and an antioxidant polymer, the flavonoid small molecules are grafted on the antioxidant polymer; the antioxidant polymer contains a boric acid group and a dihydropyrimidone structure. Solubilizing flavonoid small molecules are creatively introduced to be combined with an anti-oxidation polymer developed on the basis of Biginelli reaction, the oxidation resistance can be further enhanced, meanwhile, an immunoregulation function is achieved, and healing of diabetic wounds is effectively promoted. In addition, the preparation method of the novel antioxidant self-healing hydrogel provided by the invention is simple in process, mild in gel forming condition and mature in industrial production condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new material applications, and in particular to a hydrogel dressing for diabetic wound repair and a preparation method thereof. Background Art

[0002] At present, diabetes is a multi-faceted chronic metabolic disease that seriously affects the quality of life of patients and brings huge economic and social burdens. In clinical practice, diabetic patients often have wounds that have not healed or have no tendency to heal after more than one month of regular treatment, that is, chronic refractory wounds. Due to the high level of inflammation in diabetic wound tissues and immune dysfunction, the polarization of regenerative macrophages becomes difficult. Polymer hydrogel is a three-dimensional cross-linked network scaffold that can maintain a moist environment at the wound site and isolate bacterial infection. Dynamic boronate bonds are special chemical bonds that can break and re-form under specific conditions. This dynamic property makes boronate not a completely stable molecule, but in a state of dynamic equilibrium. Its presence can give hydrogels the characteristics of self-adaptation, thereby avoiding secondary infections caused by dressing rupture or local movement of the human body. In addition, boronate bonds can also be used to prepare gels with anti-inflammatory and antibacterial activity, and promote the expression of transforming growth factor, anti-inflammatory factor, and vascular endothelial growth factor. Flavonoids are natural metabolites unique to plants, with a wide range of sources, easy to obtain, good safety, and pharmacological effects of anti-inflammatory, antioxidant, and remodeling the immune microenvironment. The Chinese invention patent application with publication number CN201910553404.6 discloses the preparation of a self-repairing antioxidant hydrogel based on borate bonds. However, the above-mentioned material still has the problem that the antioxidant performance of the DHPM group on which it mainly relies is very limited and the skin regeneration function is not well regulated. It is urgent to develop a gel dressing with enhanced antioxidant capacity and capable of regulating the polarization of regenerative macrophages. Summary of the invention

[0003] The purpose of the present invention is to provide a hydrogel dressing for diabetic wound repair, so as to solve the technical problems of limited antioxidant capacity and poor ability to regulate polarization of regenerative macrophages in the prior art.

[0004] In order to solve the above technical problems, the present invention provides a hydrogel dressing for diabetic wound repair, comprising polyvinyl alcohol, flavonoid small molecules, and antioxidant polymers;

[0005] The flavonoid small molecules are grafted onto the antioxidant polymer;

[0006] The antioxidant polymer contains a boric acid group and a dihydropyrimidone structure.

[0007] The antioxidant property of colloid factors depends on the antioxidant capacity of the dihydropyrimidone structure (DHPM group).

[0008] Hydrogels loaded with flavonoid small molecules have excellent immune regulatory capabilities.

[0009] Preferably, the flavonoid small molecule is selected from one or more of myricetin (Mry), dihydromyricetin (2Hmry), quercetin (Que), and catechin (Cat).

[0010] The present invention also provides a method for preparing the hydrogel dressing, and the specific preparation steps are as follows:

[0011] Step 1, weighing 8-12 parts of the antioxidant polymer P1 powder, dissolving it in 100 parts of 0.01M PBS solution at room temperature, stirring at a rate of 250-400 rpm until the antioxidant polymer powder is completely dissolved, to obtain an antioxidant polymer solution;

[0012] Step 2, taking the flavonoid small molecule, adding 0.1-5 mg of the flavonoid small molecule to every 1 ml of the solution, adding the flavonoid small molecule to the antioxidant polymer solution of step 1, stirring evenly, to obtain a flavonoid-antioxidant polymer solution;

[0013] Four common flavonoid small molecules, namely catechin (Cat), quercetin (Que), myricetin (mry), and dihydromyricetin (2H mry), were placed in 0.01M PBS solution and antioxidant polymer P1 solution respectively. Figure 2 As shown, after stirring, the PBS solution loaded with flavonoid small molecules was turbid, and the marker on the back of the bottle could not be seen; while in the four flavonoid small molecules-antioxidant polymer P1 solutions, the solutions were clear and transparent, and the marker on the back of the bottle could be clearly seen, proving that the antioxidant polymer P1 solution had a good solubilizing effect on flavonoid small molecules;

[0014] Step 3, taking 6-10 parts of polyvinyl alcohol (PVA) powder, placing it in 100 parts of 0.01M PBS solution, stirring until completely dissolved, to obtain a polyvinyl alcohol solution with a concentration of 6-10wt%;

[0015] Step 4, mixing the flavonoid-antioxidant polymer solution described in step 2 with the polyvinyl alcohol solution described in step 3, and shaking for 90-150 seconds to obtain an antioxidant hydrogel (Gel-flavonoids);

[0016] The above components are all calculated by mass.

[0017] Furthermore, in step 4, the flavonoid-antioxidant polymer solution is mixed with the polyvinyl alcohol solution in a volume ratio of 1:(0.5-2).

[0018] Preferably, the volume ratio of the flavonoid-antioxidant polymer solution to the polyvinyl alcohol solution is selected from 1:0.5, 1:1, 1:1.5, 1:1.8, 1:2 and any range between any two of the above values. Preferably, the volume ratio is 1:(1-1.5)

[0019] Furthermore, the preparation steps of the antioxidant polymer powder in step 1 are as follows:

[0020] Step A, mixing ethylene glycol acetoacetate, a boric acid compound containing an aldehyde group, and a urea compound in a molar ratio of 1:1:(1-3), reacting in an organic solvent at 90-120° C. for 3-5 hours under the catalysis of a metal halide, to obtain a reaction solution containing a boric acid group and a dihydropyrimidone structure;

[0021] The amount of ethylene glycol acetoacetate methacrylate added to every 1-1.5 ml of the organic solvent is 1 mmol; preferably, the amount of ethylene glycol acetoacetate methacrylate added to every 1 ml of the organic solvent is 1 mmol.

[0022] Preferably, the molar ratio of the ethylene glycol acetoacetate, the aldehyde-containing boric acid compound and the thiourea compound may be 1:1:1.5.

[0023] Step B, the reaction solution containing a boronic acid group and a dihydropyrimidone structure in step A is precipitated with water and ether, and vacuum dried, and the monomer containing a boronic acid group and a dihydropyrimidone structure (PBA-DHPM) is obtained after collection for standby use;

[0024] Step C, taking the monomer containing a boronic acid group and a dihydropyrimidone structure obtained in the step B, mixing it with polyethylene glycol monomethyl ether methacrylate and an oil-soluble initiator in a molar ratio of 10:(10-20):(0.1-0.15), reacting in an organic solvent for 20-24 hours at a reaction temperature of 60-80° C., to obtain the antioxidant polymer P1.

[0025] The amount of the monomer containing a boronic acid group and a dihydropyrimidone structure added per 1-1.5 ml of the organic solvent is 1 mmol.

[0026] Preferably, the monomer containing a boric acid group and a dihydropyrimidone structure, polyethylene glycol monomethyl ether methacrylate, and the oil-soluble initiator are in a molar ratio of 10:10:0.1.

[0027] Preferably, the boronic acid compound containing an aldehyde group is selected from one or more of 4-formylphenylboronic acid, 4-acetylphenylboronic acid, 4-propionylphenylboronic acid, and 4-butyrylphenylboronic acid.

[0028] Preferably, the metal halide in step A is selected from one or more mixtures of magnesium chloride, magnesium bromide and magnesium iodide;

[0029] The added mass ratio of the metal halide is 15-30wt% of the ethylene glycol acetoacetate methacrylate. Preferably, the added mass ratio of the metal halide is 20wt%.

[0030] Furthermore, the organic solvent is selected from one or more of acetic acid, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0031] Furthermore, the urea compound in step A is selected from thiourea compounds and / or urea compounds.

[0032] Furthermore, the oil-soluble initiator in step C is selected from one or more of azobisisoheptanitrile, azobisisobutyronitrile, and dibenzoyl peroxide.

[0033] By adopting the above technical solution, the present invention has the following beneficial effects:

[0034] The hydrogel dressing for diabetic wound repair provided by the present invention creatively introduces solubilizing flavonoid small molecules and combines them with antioxidant polymers to further enhance antioxidant capacity, while also having immunomodulatory function, effectively promoting the healing of diabetic wounds; in addition, the preparation method of the novel antioxidant self-healing hydrogel provided by the present invention has a simple process, mild gelling conditions, and mature industrial production conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 (a) is the NMR characterization of PBA-DHPM monomer;

[0037] Figure 1(b) is the NMR characterization of the antioxidant polymer P1;

[0038] Figure 2 Schematic diagram of the solubilization effect of PBA-DHPM polymer solution on four flavonoid small molecules;

[0039] FIG3( a ) is a SEM image of the hydrogel (6 wt %) provided by the present invention;

[0040] FIG3( b ) is a SEM image of the hydrogel (7 wt %) provided by the present invention;

[0041] FIG3( c ) is a SEM image of the hydrogel (8 wt %) provided by the present invention;

[0042] Figure 4 Schematic diagram of the hydrogel self-healing process;

[0043] Figure 5 ABTS for loading flavonoids into hydrogels + ˙Schematic diagram of quenching ability test;

[0044] Figure 6 is the relationship between the modulus and strain of the 8 wt% solid content hydrogel at 25°C;

[0045] Figure 7 The graph of the modulus of 8 wt% solid content hydrogel under alternating strain (300% and 1%) at 25°C over time;

[0046] Figure 8 Schematic diagram of hydrogel self-adaptation;

[0047] FIG9( a ) is a diagram showing the cell safety evaluation of the additive-free hydrogel Gel-0;

[0048] FIG9( b ) is a diagram showing the cell safety evaluation of hydrogels loaded with four different flavonoid small molecules;

[0049] Fig.10 The PCR quantitative results of cell typing of mouse macrophage Raw264.7 after hydrogel 3D culture;

[0050] Fig.11 Schematic diagram of a representative wound healing process of a wound dressing in diabetic rats; DETAILED DESCRIPTION

[0051] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] The present invention is further explained below in conjunction with specific implementation modes.

[0053] The hydrogel dressing for diabetic wound repair provided by the present invention and the preparation method thereof are as follows:

[0054] 1. Preparation of PBA-DHPM Monomer

[0055] Ethylene glycol acetoacetate (AEMA), a boric acid compound containing an aldehyde group, and a urea compound are weighed in sequence according to a molar ratio of 1:1:(1-3).

[0056] Then weigh the metal halide, the mass ratio of which is 15-30wt% of ethylene glycol acetoacetate methacrylate, add the above four reactants into a round-bottom flask containing an organic solvent, and react in an oil bath at 100°C for 4 hours. After the reaction, the reaction solution is precipitated in cold water three times, then precipitated in ether, and finally vacuum dried to obtain the monomer M1 (PBA-DHPM) containing a boronic acid group and a dihydropyrimidone structure.

[0057] 2. Preparation of PBA-DHPM Polymer

[0058] The above M1 monomer was mixed with polyethylene glycol monomethyl ether methacrylate (PEGMA) and an oil-soluble initiator in a molar ratio of 10:(10-20):(0.1-0.15), added to an organic solvent, sealed with a rubber septum, blown with nitrogen for 30 minutes, and then reacted in an oil bath at 70°C for 24 hours. The reaction solution was precipitated in ether three times and then vacuum dried to obtain pure PBA-DHPM polymer P1.

[0059] 3. Preparation of Hydrogel

[0060] A 0.01M commercial PBS solution (pH 7.4) was heated to about 70°C, and PVA (0588) powder was added at a mass ratio of 6wt%-10wt%, and stirred overnight to obtain a PBS solution of PVA with a mass concentration of 6-10wt%. A series of flavonoid compounds were dissolved in the antioxidant polymer P1 solution to prepare the P1-flavonoid solution.

[0061] The PBS solution of PVA with a mass concentration of 6-10 wt% and the P1-flavonoid solution were mixed in equal volumes to prepare a hydrogel loaded with flavonoids.

[0062] The study found that the hardness of the hydrogel can be adjusted by adjusting the mass concentration of the PVA-PBS solution; at the same time, adding different types and proportions of flavonoid small molecules has a certain effect on the antioxidant properties of the hydrogel.

[0063] Example 1

[0064] As shown in Figure 1(a), Figure 1(b) and Figure 4 As shown, this example provides the preparation of antioxidant polymer P1 and flavonoid small molecule loaded hydrogel.

[0065] 1. Preparation of PBA-DHPM Monomer

[0066] 16.05 g of ethylene glycol acetoacetate (AEMA), 11.25 g of 4-formylphenylboronic acid, 8.55 g of thiourea and 1.43 g of magnesium chloride (MgCl2) were weighed and added to a round-bottom flask containing 75 mL of acetic acid, and reacted in an oil bath at 100 ° C for 4 hours. After the reaction, the reaction solution was precipitated in cold water three times, then precipitated in ether, and finally vacuum dried to obtain a monomer (PBA-DHPM) containing a boronic acid group and a dihydropyrimidone structure. As shown in Figure 1 (a) 1H-NMR spectrum, the target PBA-DHPM monomer (M1) was obtained in this example.

[0067] 2. Preparation of PBA-DHPM Polymer

[0068] 20.2g of M1 monomer was mixed with 47.5g of polyethylene glycol monomethyl ether methacrylate (PEGMA), 0.125g of azobisisoheptanenitrile (ABVN) and 50ml of N,N-dimethylformamide (DMF), sealed with a rubber diaphragm, blown with nitrogen flow for 30 minutes, and then reacted in a 70°C oil bath for 24 hours. The reaction solution was precipitated in ether three times and then vacuum dried to obtain pure PBA-DHPM polymer P1. As shown in the 1H-NMR spectrum of Figure 1(b), the characteristic peaks indicate that the target antioxidant polymer P1 was successfully obtained in this example.

[0069] 3. Preparation of Hydrogel

[0070] A 0.01M commercial PBS solution (pH 7.4) was heated to about 70°C, and a certain amount of PVA (0588) powder was added and stirred overnight to obtain a PBS solution of PVA with a mass concentration of 7%. A series of flavonoid compounds (5 mg) were dissolved in an antioxidant polymer P1 solution (8 wt%, 10 mL) to prepare a P1-flavonoid solution. The two components were mixed in equal volumes to prepare a hydrogel Gel1 loaded with flavonoids.

[0071] like Figure 4 As shown, the prepared hydrogel is divided into two parts and then put together again. After 3 hours, the boundary between the two parts of the hydrogel is blurred and a hydrogel as a whole can be formed. Most of the traditional wound dressing materials on the market do not have self-healing properties.

[0072] Example 2

[0073] like Figure 3(a)-Figure 3(c) As shown, this example verifies the effect of different amounts of polyvinyl alcohol added on the properties of the reaction product hydrogel.

[0074] The preparation method of the hydrogel loaded with flavonoid small molecules in this example is basically the same as that in Example 1, except that three PBS solutions of PVA with mass concentrations of 6wt%, 7wt%, and 8wt% are used to prepare three hydrogel samples Gel-6, Gel-7, and Gel-8, respectively. Figure 3(a)-Figure 3(c) As shown, it can be clearly seen that as the mass concentration of the PVA PBS solution increases, the resulting hydrogel structure becomes denser and the macroscopic hardness of the hydrogel becomes greater. Therefore, after multiple experimental verifications, the mass concentration of the PVA PBS solution is preferably 6-10wt%.

[0075] Example 3

[0076] This example verifies the antioxidant capacity of the hydrogel loaded with flavonoid small molecules.

[0077] Step 1: Mix 400uL of 10wt% PVA solution with 172uL of ABTS with an absorbance of 3. + ˙The solutions were mixed to obtain 7 wt% PVA-ABTS with an absorbance of 3 and a pH of 7.4. + ˙Solution;

[0078] Step 2: Continue to dilute the 7 wt % PVA-ABTS with 7 wt % PVA solution + ˙The solution was heated to an absorbance of 1.

[0079] Step 3: Four different flavonoid small molecule-antioxidant polymer solutions were used to react with PVA-ABTS + ˙Equal volumes of the solutions were mixed to obtain a solution containing ABTS + ˙Hydrogel, labeled with Cat (catechin), Que (quercetin), Mry (myricetin), 2H myr (dihydromyricetin); PBS solution and PVA-ABTS + ˙Equal volumes of the solutions were mixed as the blank control group Gel.

[0080] Step 4: Take photos of the five groups of comparative experimental hydrogels during mixing and after mixing for 1 minute. Figure 5 As shown in the figure, it can be clearly seen that the color of the hydrogel in the blank control group Gel is darker after mixing for 1 minute, while the colors of the hydrogels in the other four groups with different flavonoid small molecules added are obviously lighter, proving that ABTS + ˙It was effectively removed, which verified that flavonoids have a significant effect on improving antioxidant capacity. The hydrogel loaded with flavonoid small molecules provided by the present invention has excellent antioxidant capacity.

[0081] Example 4

[0082] like Figure 6As shown, this example verifies the strain bearing capacity of the hydrogel loaded with flavonoid small molecules.

[0083] The preparation method of the hydrogel loaded with flavonoid small molecules in this embodiment is basically the same as that in Example 1, except that acetoacetic acid methacrylate (AEMA), 4-acetylphenylboronic acid and urea are mixed in a molar ratio of 1:1:3 in the preparation process of PBA-DHPM monomer, and PBA-DHPM monomer M2 is prepared under the catalysis of magnesium iodide. The subsequent steps are the same as those in Example 1, and the hydrogel Gel2 loaded with flavonoid small molecules is prepared.

[0084] At 25°C, different strains were applied to the flavonoid-loaded hydrogel Gel2, and the G' and G" values ​​were recorded (frequency = 1 Hz). Figure 6 As shown, when the strain exceeded 80%, the network structure of hydrogel Gel2 was completely destroyed.

[0085] Example 5

[0086] like Figure 7 As shown, this example verifies the rheological properties of the hydrogel loaded with flavonoid small molecules.

[0087] The preparation method of the hydrogel loaded with flavonoid small molecules in this example is basically the same as that in Example 1, except that, during the preparation of the PBA-DHPM polymer, 20.2 g of M1 monomer was mixed with 95 g of polyethylene glycol monomethyl ether methacrylate (PEGMA), 0.125 g of dibenzoyl peroxide (BPO) and 50 ml of N,N-dimethylacetamide (DMAC), and the subsequent steps were the same as in Example 1 to prepare the flavonoid-loaded hydrogel Gel3.

[0088] like Figure 7 As shown in the figure, the modulus of the 8wt% solid content hydrogel changes with time under alternating strain (300% and 1%) at 25°C. The hydrogel did not break under 1% strain, and the hydrogel completely broke under 300% strain. At 300% strain, after each complete destruction, the hydrogel network recovered to its original strength under 1% strain. This verifies that the hydrogel loaded with flavonoid small molecules has good rheological properties.

[0089] Example 6

[0090] like Figure 8 As shown, this example verifies the self-healing ability of the hydrogel loaded with flavonoid small molecules.

[0091] The preparation method of the hydrogel loaded with flavonoid small molecules in this example is basically the same as that in Example 1, except that, during the preparation of the PBA-DHPM monomer, 16.05 g of ethylene glycol acetoacetate (AEMA), 11.25 g of 4-butyrylphenylboronic acid, 17.1 g of thiourea and 2.15 g of magnesium chloride (MgCl2) were added to 75 mL of acetonitrile solution for reaction, and the subsequent steps were the same as those in Example 1 to prepare the flavonoid-loaded hydrogel Gel4.

[0092] 3 ml of Gel4 hydrogel was dyed blue and injected into a T-shaped mold through a 22-gauge needle. After 6 hours, the hydrogel completely conformed to the mold and adapted to a T shape. The hydrogel was then re-injected into the H-shaped and U-shaped molds for remodeling. The adaptive process of the hydrogel was monitored by taking pictures. Figure 8 As shown, after a period of remodeling, the Gel4 hydrogel can adapt well to the shape of the mold, thereby verifying that the hydrogel loaded with flavonoid small molecules provided by the present invention has excellent self-adaptation ability and can adapt to wounds of different shapes and sizes.

[0093] Example 7

[0094] like Figure 9(a)-Figure 10 As shown, this example verifies the cell safety and immune regulation effect by comparing the culture results of mouse macrophages loaded with hydrogels of different types of flavonoid small molecules.

[0095] RAW264.7 was resuspended in PVA solution at a density of 2 million cells / ml, and mixed with equal volumes of four different flavonoid small molecule-antioxidant polymer solutions containing catechin, quercetin, myricetin and dihydromyricetin, respectively, and cultured in an incubator at 37°C, 5% CO2 for 24 hours to obtain four hydrogels loaded with different flavonoid small molecules, which were labeled as Gel-Cat, Gel-Que, Gel-Mry, and Gel-2H myr, respectively; in addition, an antioxidant polymer solution without flavonoid small molecules was mixed with the above PVA solution in equal volumes to prepare hydrogel Gel-0 as a blank control group.

[0096] The cell viability of the above five groups of samples was detected using a fluorescent live / dead viability assay kit (KeyGEN Bio TECH), that is, 2μM calcein (AM) and 8μM propidium iodide (PI) staining solution were incubated with the cells for 30 minutes and then observed under a fluorescence microscope. As shown in Figure 9, the cells in each group of hydrogels can maintain good activity, the survival rate is significantly higher, and the morphology is normal, thereby verifying that the hydrogel provided by the present invention has excellent cell safety.

[0097] PCR quantitative detection was performed on the cell typing of mouse macrophage Raw264.7 cultured in the five groups of hydrogels in this example. The total RNA of RAW264.7 was extracted using TRIzol reagent, and then cDNA was obtained through reverse transcription. Finally, the following genes were amplified: ccr7, il6, inos, il10, arg1 and gapdh. After PCR quantitative detection, the results are as follows Fig.10 As shown, compared with the blank control group Gel-0, the expression of pro-inflammatory M1 differentiation markers ccr7, il6 and inos in macrophages cultured in each group of hydrogels loaded with flavonoids was significantly reduced; the expression of anti-inflammatory M2 differentiation markers il10 and arg1 was significantly increased. In summary, hydrogels loaded with flavonoid small molecules have a positive effect on inhibiting the occurrence of inflammation at the wound, can effectively regulate the immune microenvironment at the wound, reduce the occurrence of inflammation, and promote wound healing.

[0098] Example 8

[0099] like Fig.11 As shown, this example verifies the repair effect of the use of hydrogel excipients loaded with flavonoid small molecules on diabetic wounds by continuous monitoring of different dressings on diabetic rat wounds for 21 days.

[0100] The diabetic model was established by injecting streptozotocin at a dose of 60 mg / kg into 9-week-old SD rats. The model was considered successful when the blood glucose level was higher than 16.7 mmol / L after one week.

[0101] Skin defects with a diameter of 8 mm were created on the backs of diabetic rats, and the wounds were treated according to the following groups: NC (no dressing), 3M, Gelma (Engineering For Life), Gel, Gel-myricetin, Gel-dihydromyricetin, Gel-catechin, Gel-quercetin. The wounds treated with each dressing were photographed and compared on days 0, 3, 7, and 14. The results are shown in Figure 2. Fig.11 As shown, the wound healing speed of each group using hydrogel dressings was significantly faster than that of the other three groups using other dressings. Among the groups using various hydrogel dressings, the wound healing effect of each group using hydrogel dressings loaded with flavonoid small molecules was better. In summary, hydrogel dressings loaded with flavonoid small molecules have a significant promoting effect on diabetic wound healing and repair.

[0102] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A hydrogel dressing for diabetic wound repair, characterized in that: Contains polyvinyl alcohol, flavonoid small molecules, and antioxidant polymers; The flavonoid small molecules are grafted onto the antioxidant polymer; The antioxidant polymer contains a boric acid group and a dihydropyrimidone structure.

2. The hydrogel dressing according to claim 1, characterized in that The flavonoid small molecules are selected from one or more of myricetin, dihydromyricetin, quercetin and catechin.

3. A method for preparing the hydrogel dressing according to claim 1, characterized in that: The preparation steps are as follows: Step 1, weighing 8-12 parts of the antioxidant polymer powder, dissolving it in 100 parts of 0.01M PBS solution at room temperature, and stirring until the antioxidant polymer powder is completely dissolved to obtain an antioxidant polymer solution; Step 2, taking the flavonoid small molecule, adding 0.1-5 mg of the flavonoid small molecule to every 1 ml of the solution, adding the flavonoid small molecule to the antioxidant polymer solution of step 1, stirring evenly, to obtain a flavonoid-antioxidant polymer solution; Step 3, taking 6-10 parts of polyvinyl alcohol powder, placing it in 100 parts of 0.01M PBS solution, stirring until completely dissolved, to obtain a polyvinyl alcohol solution with a concentration of 6-8wt%; Step 4, taking the flavonoid-antioxidant polymer solution described in step 2 and the polyvinyl alcohol solution described in step 3 and shaking and mixing them to obtain an antioxidant hydrogel; The above components are all calculated by mass.

4. The preparation method according to claim 3, characterized in that: Step 4: The flavonoid-antioxidant polymer solution and the polyvinyl alcohol solution are mixed in a volume ratio of 1:0.5-2.

5. The preparation method according to claim 3, characterized in that: The preparation steps of the antioxidant polymer powder in step 1 are as follows: Step A, ethylene glycol acetoacetate, a boric acid compound containing an aldehyde group, and a urea compound are mixed in a molar ratio of 1:1:1-3, and reacted in an organic solvent at 90-120° C. for 3-5 hours under the catalysis of a metal halide to obtain a reaction solution containing a boric acid group and a dihydropyrimidone structure; The amount of ethylene glycol acetoacetate methacrylate added to each 1-1.5 ml of the organic solvent is 1 mmol; Step B, the reaction solution containing a boronic acid group and a dihydropyrimidone structure in step A is precipitated with water and ether, and vacuum dried, and the monomer containing a boronic acid group and a dihydropyrimidone structure is collected for standby use; Step C, taking the monomer containing a boronic acid group and a dihydropyrimidone structure obtained in the step B, mixing it with polyethylene glycol monomethyl ether methacrylate and an oil-soluble initiator in a molar ratio of 10:10-20:0.1, reacting in an organic solvent for 20-24 hours at a reaction temperature of 60-80° C. to obtain the antioxidant polymer; The amount of the monomer containing a boronic acid group and a dihydropyrimidone structure added per 1-1.5 ml of the organic solvent is 1 mmol.

6. The preparation method according to claim 5, characterized in that: The boronic acid compound containing an aldehyde group is selected from one or more of 4-formylphenylboronic acid, 4-acetylphenylboronic acid, 4-propionylphenylboronic acid, and 4-butyrylphenylboronic acid.

7. The preparation method according to claim 5, characterized in that: The metal halide in step A is selected from one or more mixtures of magnesium chloride, magnesium bromide and magnesium iodide; The added mass ratio of the metal halide is 15-30wt% of the ethylene glycol acetoacetate and methacrylate.

8. The preparation method according to claim 5, characterized in that: The organic solvent is selected from one or more of acetic acid, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, and N,N-dimethylacetamide.

9. The preparation method according to claim 5, characterized in that: The urea compound in step A is selected from thiourea and / or urea compounds.

10. The preparation method according to claim 5, characterized in that: The oil-soluble initiator in step C is selected from one or more of azobisisoheptanenitrile, azobisisobutyronitrile and dibenzoyl peroxide.