Preparation method and equipment for hydrogen reduction lattice sulfur activation and regeneration of metal sulfide mercury adsorbent

The method of activating lattice sulfur and regenerating metal sulfide mercury adsorbent through hydrogen reduction solves the problems of low efficiency of mercury adsorbent and easy poisoning and deactivation in the existing technology, achieves high-efficiency mercury adsorption and long-term regeneration of adsorbent, and reduces the cost of mercury adsorbent. reduce energy consumption and costs.

CN118718977AActive Publication Date: 2024-10-01SHANGHAI UNIV OF ENG SCI

Patent Information

Application Number
CN202411017000.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-01
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Existing mercury adsorbents have low efficiency in removing gaseous zero-valent mercury (Hg0), and are easily deactivated by SO2 poisoning, making it difficult to achieve efficient regeneration and long-term use.

Method used

The preparation method of hydrogen reduction lattice sulfur activation and regeneration of metal sulfide mercury adsorbent is adopted. The mercury-sulfur bond is activated through hydrogen high-temperature reduction and regeneration treatment to generate a reducing sulfur intermediate and undergo an in-situ reverse disproportionation reaction with SO2 to remove the adsorbent surface. Sulfate to achieve reactivation and regeneration of adsorbents.

Benefits of technology

It significantly improves the mercury adsorption capacity and efficiency, extends the service life of the adsorbent, reduces energy consumption and costs, and avoids the poisoning and deactivation of the adsorbent by SO2, achieving low-temperature mercury analysis and recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718977A_ABST
    Figure CN118718977A_ABST
Patent Text Reader

Abstract

Hydrogen is adopted to react on the surface of metal sulfide to generate a reducing sulfur intermediate, the reducing sulfur intermediate and sulfur dioxide in flue gas are subjected to an in-situ reverse disproportionation reaction to generate an active sulfur substance for flue gas mercury adsorption, the adsorbent saturated in adsorption is subjected to high-temperature reduction in a hydrogen atmosphere so as to effectively analyze mercury, and the step of activating the adsorbent is repeated, so that the mercury content in the flue gas is effectively reduced. Sulfate on the surface of the adsorbent is effectively removed, toxic interference of sulfur dioxide in flue gas and the sulfate on the surface of the adsorbent on active sites is avoided, the mercury adsorbent is regenerated, the mercury adsorption capacity is greatly improved, energy consumption is reduced, meanwhile, the service life of the adsorbent is prolonged, the use amount of the adsorbent is reduced, and cost is saved. The method can be widely applied to the mercury adsorption field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental protection, and in particular to a preparation method and equipment for a hydrogen-reduced lattice sulfur-activated and regenerated metal sulfide mercury adsorbent. Background Art

[0002] Mercury is a toxic element that is persistent, bioaccumulative, highly toxic and mobile in the atmospheric environment, and poses a great threat to the ecological environment and human health. Existing wet flue gas desulfurization equipment and electrostatic precipitator equipment can effectively remove divalent mercury (Hg 2+ ) and particulate mercury (Hgp), while gaseous zero-valent mercury (Hg 0 ) is much more difficult to remove.

[0003] Adsorption is the removal and recovery of Hg from gaseous environments 0 The most promising method. Currently used adsorbents include activated carbon, fly ash, metals and metal oxides. However, traditional mercury adsorbents generally have problems such as low adsorption efficiency and low capacity. The metal sulfide adsorbents currently used in cutting-edge research have excellent adsorption performance, but they also have problems such as low capacity and easy deactivation. In addition, SO2 and other gases are also produced in coal burning, smelting, and chemical industries along with Hg 0 When emitted together, SO2 will poison and deactivate most adsorbents, thereby reducing the mercury adsorption activity.

[0004] Therefore, a green and environmentally friendly method is currently needed to solve the sulfate poisoning on the adsorbent surface and eliminate the negative impact of SO2 in sulfur-containing flue gas. Summary of the invention

[0005] The purpose of the present invention is to solve the deficiencies of the above-mentioned technology and to provide a preparation method and equipment for activating and regenerating metal sulfide mercury adsorbent by reducing lattice sulfur with hydrogen. The method is suitable for the activation and regeneration process of the metal sulfide adsorbent in the adsorption and purification process of sulfur-containing mercury flue gas.

[0006] To this end, the present invention provides a method for preparing a hydrogen-reduced lattice sulfur activated and regenerated metal sulfide mercury adsorbent, characterized in that it comprises the following steps:

[0007] (1) Mercury adsorption process:

[0008] Passing the sulfur-containing mercury flue gas into an adsorption furnace filled with a metal sulfide mercury adsorbent, so that the mercury in the flue gas is captured by the metal sulfide mercury adsorbent in the adsorption furnace;

[0009] (2) Adsorbent regeneration process:

[0010] The metal sulfide mercury adsorbent saturated with mercury adsorption in step (1) is subjected to high-temperature reduction and regeneration treatment by passing hydrogen gas to activate the mercury-sulfur bond and achieve mercury desorption;

[0011] (3) Adsorbent reactivation process:

[0012] Passing hydrogen and sulfur-containing mercury flue gas into the metal sulfide mercury adsorbent after mercury desorption in step (2), so that the hydrogen activates the lattice sulfur sites on the surface of the metal sulfide mercury adsorbent to react and generate a reduced sulfur intermediate, and the reduced sulfur intermediate reacts with sulfur dioxide in the flue gas to generate an active sulfur substance in situ, so that the surface of the metal sulfide mercury adsorbent is activated, and a mercury adsorption process is repeated;

[0013] During the regeneration and reactivation process of the adsorbent, hydrogen reacts with sulfate generated on the surface of metal sulfides, reducing them to active sulfur substances and reducing sulfur intermediates, effectively removing sulfate from the surface of the adsorbent and avoiding poisoning and inactivation of the active sites of metal sulfides.

[0014] The main reactions involved in the process are as follows:

[0015] Mercury adsorption process:

[0016] Active sulfur substances + Hg 0 →HgS

[0017] SO2+O2+metal sulfide→sulfate

[0018] Adsorbent regeneration process:

[0019] H2+HgS→Hg 0 +Reduced sulfur intermediates

[0020] H2 + metal sulfide lattice sulfur → reduced sulfur intermediate (secondary reaction)

[0021] H2+sulfate→reduced sulfur intermediate+active sulfur species+H2O

[0022] Adsorbent reactivation process:

[0023] H2 + metal sulfide lattice sulfur → reduced sulfur intermediate

[0024] Reducing sulfur intermediate + SO2 → active sulfur species

[0025] H2+sulfate→reduced sulfur intermediate+active sulfur species+H2O

[0026] Repeat the cycle...

[0027] Preferably, the metal sulfide is a chalcophilic or siderophilic element sulfide.

[0028] Preferably, the metal sulfide is at least one of copper sulfide, zinc sulfide, molybdenum sulfide and cobalt sulfide.

[0029] Preferably, the hydrogen concentration used in the adsorbent regeneration process is in the range of 10-5000 ppm and the reaction temperature is 100-600°C.

[0030] Preferably, the hydrogen concentration used in the adsorbent reactivation process is in the range of 10-5000 ppm and the reaction temperature is 100-600°C.

[0031] An apparatus for implementing the above-mentioned preparation method of hydrogen reduction lattice sulfur activation and regeneration metal sulfide mercury adsorbent comprises two adsorption furnaces and a six-way valve, wherein the two adsorption furnaces are respectively adsorption furnace I and adsorption furnace II, and the six-way valve is provided with an air inlet valve I, an air inlet valve II, an air inlet valve IV, an air inlet valve V and an air outlet valve III and an air outlet valve VI, the adsorption furnace I is arranged on a pipeline connected between the air outlet valve VI and the air inlet valve V, and a three-way valve VII is further provided on the pipeline between the adsorption furnace I and the air inlet valve V, the adsorption furnace II is arranged on a pipeline connected between the air outlet valve III and the air inlet valve IV, and a three-way valve VIII is further provided on the pipeline between the adsorption furnace II and the air inlet valve IV.

[0032] The process route is divided into three processes. In order to realize these three processes, two tubular adsorption furnaces are used together, as follows:

[0033] Preferably, during the mercury adsorption process, the inlet valve II is opened to introduce sulfur-containing mercury flue gas, and then the outlet valve VI, the three-way valve VII, the inlet valve V, and the outlet valve III are opened in sequence, and the sulfur-containing mercury flue gas flows along the route of the inlet valve II→the outlet valve VI→the three-way valve VII→the inlet valve V→the outlet valve III, and passes through the adsorption furnace I and the adsorption furnace II in sequence, so that the mercury in the flue gas is captured by the mercury adsorbent in the adsorption furnace. The three-way valve VII is connected to the pipeline between the adsorption furnace I and the inlet valve V.

[0034] Preferably, during the adsorbent regeneration process, the air inlet valve I is opened to introduce hydrogen, the air outlet valve VI is opened to allow the hydrogen to pass through the adsorption furnace I, and the furnace temperature is increased to desorb and regenerate the adsorbent. This process can effectively activate the mercury-sulfur bond and achieve mercury desorption.

[0035] Preferably, during the adsorbent reactivation process, the inlet valve I and the inlet valve II are opened, hydrogen and sulfur-containing mercury flue gas are introduced, and the outlet valve VI, the three-way valve VII, the inlet valve V and the outlet valve III are opened, so that the airflow flows along the route of the inlet valve II→the outlet valve VI→the three-way valve VII→the inlet valve V→the outlet valve III, and the hydrogen and the sulfur-containing mercury flue gas are sequentially passed through the adsorption furnace I and the adsorption furnace II to perform in-situ reactivation of the adsorbent by reverse disproportionation. In this process, hydrogen can effectively activate lattice sulfur and activate metal-sulfur sites, and hydrogen can react with sulfate on the surface of the adsorbent at high temperature to reduce it to active sulfur substances and reducing sulfur intermediates, thereby removing sulfate and avoiding poisoning and inactivation of metal sulfide active sites.

[0036] Both tubular adsorption furnaces in the process route can be used for mercury adsorption, which is mainly controlled by the valve opening and closing sequence of the six-way valve. In the process route of the present invention, the mercury adsorption and adsorbent reactivation processes pass through two tubular adsorption furnaces, and the adsorbent regeneration process only passes through the tubular adsorption furnace that needs to be regenerated.

[0037] The present invention provides a preparation method and equipment for activating and regenerating a metal sulfide mercury adsorbent based on hydrogen reduction of lattice sulfur, which has the following beneficial effects:

[0038] (1) The metal sulfide surface is activated by a trace amount of hydrogen, which reacts with SO2 in the flue gas in situ to undergo an in-situ reverse disproportionation reaction, thereby converting SO2 into active sulfur substances for mercury adsorption, greatly improving the mercury adsorption capacity and reducing the toxic effects of SO2 in sulfur-containing mercury flue gas. At the same time, hydrogen activation will not release toxic and harmful gases.

[0039] (2) During the high-temperature regeneration process, the presence of trace amounts of hydrogen can effectively activate the mercury-sulfur bond and decompose mercury. Hydrogen can also effectively remove sulfate from the surface of the adsorbent, avoid poisoning and inactivation of metal sulfide active sites, continuously form active sites on the adsorbent surface, lower the regeneration temperature, significantly reduce energy consumption, and achieve low-temperature mercury decomposition and recovery.

[0040] (3) The adsorption efficiency of the activated adsorbent is greatly improved, and it can be regenerated and recycled, which greatly increases the service life of the adsorbent and reduces the amount of adsorbent used, saving costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 The present invention is a schematic diagram of the process flow of the preparation process of the hydrogen reduction lattice sulfur activation and regeneration metal sulfide mercury adsorbent.

[0042] In the figure: 1. Inlet valve I; 2. Inlet valve II; 3. Exit valve III; 4. Inlet valve IV; 5. Inlet valve V; 6. Exit valve VI; 7. Three-way valve VII; 8. Three-way valve VIII. DETAILED DESCRIPTION

[0043] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments to help understand the content of the present invention. The methods used in the present invention are all conventional methods unless otherwise specified; the raw materials and devices used are all conventional commercial products unless otherwise specified.

[0044] like Figure 1 As shown, the process route is divided into three processes, as follows:

[0045] Mercury adsorption process:

[0046] Open the air inlet valve II2 to let in the sulfur-containing mercury flue gas, then open the outlet valve VI6, the three-way valve VII7, the air inlet valve V5, and the outlet valve III3 in sequence, and the sulfur-containing mercury flue gas flows along the route of air inlet valve II2→outlet valve VI6→three-way valve VII7→inlet valve V5→outlet valve III3, and passes through the adsorption furnace I and the adsorption furnace II in sequence, so that the mercury in the flue gas is captured by the mercury adsorbent in the adsorption furnace. And the three-way valve VII7 is connected to the pipeline between the adsorption furnace I and the air inlet valve V.

[0047] Adsorbent regeneration process:

[0048] Open the air inlet valve Ⅰ1 to introduce hydrogen, open the air outlet valve VI6 to allow hydrogen to pass through the adsorption furnace Ⅰ, and increase the furnace temperature to desorb and regenerate the adsorbent.

[0049] Adsorbent reactivation process:

[0050] Open the air inlet valve Ⅰ1 and the air inlet valve II2, introduce hydrogen and sulfur-containing mercury flue gas, open the air outlet valve VI6, the three-way valve VII7, the air inlet valve V5 and the air outlet valve III3, so that the air flow flows along the route of air inlet valve II2→air outlet valve VI6→three-way valve VII7→air inlet valve V5→air outlet valve III3, and the hydrogen and sulfur-containing mercury flue gas pass through the adsorption furnace Ⅰ and the adsorption furnace II in turn to carry out reverse disproportionation and in-situ reactivation of the adsorbent.

[0051] Embodiment 1:

[0052] In the pilot test, the alumina-loaded copper sulfide adsorbent was first synthesized by a hydrothermal method using alumina (3-5 mm) pellets as the substrate and copper sulfide as the active component of the adsorbent. The synthesis amount was 10 kg and the copper sulfide loading was 10 wt%. The synthesized adsorbent was loaded into two tubular furnaces, with 5 kg of adsorbent loaded into adsorption furnace I and adsorption furnace II respectively, and a mercury adsorption experiment was carried out. The mercury concentration in the flue gas component was 1.2 mg / m 3 , SO2 concentration is 3000ppm, oxygen concentration is 5%. The reaction conditions are set at a reaction temperature of 80 degrees Celsius and a space velocity of 80000h -1. In the mercury adsorption stage, adsorption furnace I and adsorption furnace II are connected in series, and the initial mercury adsorption rate of adsorption furnace I is 99.8%, and the mercury adsorption rate of adsorption furnace II is 100%. After 24 hours, the mercury adsorption rate of adsorption furnace I dropped to 96.2%, and the mercury adsorption rate of adsorption furnace II remained 100%. After 168 hours, the mercury adsorption rate of adsorption furnace I was 63.1%, and the mercury adsorption rate of adsorption furnace II was 99.5%. In the adsorbent regeneration stage, in order to regenerate the adsorbent in adsorption furnace I, the flue gas was turned off, the hydrogen pipeline was opened, and the connection between adsorption furnace I and adsorption furnace II was disconnected. 500ppm of hydrogen was introduced into adsorption furnace I, and the temperature of adsorption furnace I was raised to 400 degrees Celsius, with a heating rate of 10 degrees per minute, and the temperature was maintained at 400 degrees for 1 hour to regenerate the mercury adsorbent. In the adsorbent reactivation stage, the flue gas pipeline was opened, and adsorption furnace I and adsorption furnace II were reconnected in series, and the temperature of adsorption furnace II was raised to 300 degrees Celsius. Flue gas and 500ppm concentration of hydrogen were introduced into the adsorption furnace I for reactivation, and the activation time was maintained for 1 hour. The activated adsorbent continued to repeat the mercury adsorption experiment. The results showed that the initial mercury adsorption efficiency of adsorption furnace I was 99.87%, and the adsorption rate of adsorption furnace II was 100%. After 24 hours, the mercury adsorption rate of adsorption furnace I was 98.9%, and the mercury adsorption rate of adsorption furnace II remained 100%. After 168 hours, the mercury adsorption rate of adsorption furnace I was 72.3%, and the mercury adsorption rate of adsorption furnace II was 98.2%. It has been verified that in-situ activation by sulfur reverse disproportionation can effectively improve the mercury adsorption efficiency and realize the regeneration of in-situ mercury adsorbent.

[0053] Embodiment 2:

[0054] The waste flue gas from a smelter was treated with mercury adsorption. First, alumina (4-8mm) pellets were used as the substrate and zinc sulfide was used as the active component of the adsorbent to synthesize an alumina-loaded zinc sulfide adsorbent by a hydrothermal method. The synthesis amount was 20 kg and the zinc sulfide loading amount was 15wt%. The synthesized adsorbent was loaded into two tubular furnaces, with 10 kg of adsorbent loaded into adsorption furnace I and adsorption furnace II respectively, for flue gas mercury adsorption treatment. The sulfur-containing mercury flue gas emitted by the smelter was taken as the treatment object. The mercury concentration in the flue gas component was 0.9 mg / m 3 , SO2 concentration is 5000ppm, oxygen concentration is 7%. The reaction conditions are set as tube furnace reaction temperature 100 degrees Celsius, space velocity 120000h -1. In the adsorption stage, adsorption furnace I and adsorption furnace II are connected in series, and the initial mercury adsorption rate of adsorption furnace I is 99.6%, and the mercury adsorption rate of adsorption furnace II is 100%. After 24 hours, the mercury adsorption rate of adsorption furnace I dropped to 96.0%, and the mercury adsorption rate of adsorption furnace II remained 100%. After 168 hours, the mercury adsorption rate of adsorption furnace I was 62.5%, and the mercury adsorption rate of adsorption furnace II was 99.2%. In the adsorbent regeneration stage, in order to regenerate the adsorbent in adsorption furnace I, the flue gas was turned off, the hydrogen pipeline was opened, and the connection between adsorption furnace I and adsorption furnace II was disconnected. 800ppm of hydrogen was introduced into adsorption furnace I, and the temperature of adsorption furnace I was raised to 400 degrees Celsius, with a heating rate of 10 degrees per minute, and the temperature was maintained at 400 degrees for 1 hour to regenerate the mercury adsorbent. In the adsorbent reactivation stage, the flue gas pipeline was opened, and adsorption furnace I and adsorption furnace II were reconnected in series, and the temperature of adsorption furnace II was raised to 350 degrees Celsius. Flue gas and 600ppm concentration of hydrogen were introduced into adsorption furnace I for reactivation, and the activation time was maintained for 1 hour. The above mercury adsorption-regeneration-activation process was repeated a total of 3 times. After three activation operations, the adsorbent was subjected to mercury adsorption treatment test experiments again. The results showed that the initial mercury adsorption efficiency of adsorption furnace I was 97.6%, and the adsorption rate of adsorption furnace II was 100%. After 24 hours, the mercury adsorption rate of adsorption furnace I was 98.9%, and the mercury adsorption rate of adsorption furnace II remained at 99.8%. After 168 hours, the mercury adsorption rate of adsorption furnace I was 70.6%, and the mercury adsorption rate of adsorption furnace II was 97.2%. It has been verified that after three in-situ activations by sulfur reverse disproportionation, the activity of the adsorbent only decreased by about 2% after repeated use.

[0055] In summary, the present invention provides suitable reaction conditions in a tubular adsorption furnace so that hydrogen reacts on the surface of the metal sulfide to generate a reducing sulfur intermediate, and then the reducing sulfur intermediate undergoes an in-situ reverse disproportionation reaction with sulfur dioxide in the flue gas to generate an active sulfur substance for flue gas mercury adsorption. The adsorbent saturated with adsorption is reduced at high temperature in a hydrogen atmosphere to effectively resolve mercury, and the adsorbent activation step is repeated to effectively remove sulfates on the surface of the adsorbent, thereby avoiding the poisoning interference of sulfur dioxide in the flue gas and sulfates on the surface of the adsorbent on the active sites to regenerate the mercury adsorbent. The sulfur-mercury flue gas adsorbed by the device can fully meet the national mercury emission requirements, and after the adsorption is completed, the sulfur and mercury resources can be recycled to obtain additional economic value products. In addition, the used adsorbent can also be regenerated for reuse by removing sulfates and generating new active sulfur sites through a surface activation method.

[0056] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a hydrogen-reduced lattice sulfur activated and regenerated metal sulfide mercury adsorbent, characterized in that: The following steps are involved: (1) Mercury adsorption process: Passing the sulfur-containing mercury flue gas into an adsorption furnace filled with a metal sulfide mercury adsorbent, so that the mercury in the flue gas is captured by the metal sulfide mercury adsorbent in the adsorption furnace; (2) Adsorbent regeneration process: The metal sulfide mercury adsorbent saturated with mercury adsorption in step (1) is subjected to high-temperature reduction and regeneration treatment by passing hydrogen gas to activate the mercury-sulfur bond and achieve mercury desorption; (3) Adsorbent reactivation process: Passing hydrogen and sulfur-containing mercury flue gas into the metal sulfide mercury adsorbent after mercury desorption in step (2), so that the hydrogen activates the lattice sulfur sites on the surface of the metal sulfide mercury adsorbent to react and generate a reduced sulfur intermediate, and the reduced sulfur intermediate reacts with sulfur dioxide in the flue gas to generate an active sulfur substance in situ, so that the surface of the metal sulfide mercury adsorbent is activated, and a mercury adsorption process is repeated; During the regeneration and reactivation of the adsorbent, hydrogen reacts with sulfate generated on the surface of metal sulfides, reducing them to active sulfur substances and reducing sulfur intermediates, effectively removing sulfate from the adsorbent surface and avoiding poisoning of the active sites of metal sulfides.

2. The method for preparing a hydrogen reduction lattice sulfur activation and regeneration metal sulfide mercury adsorbent according to claim 1, characterized in that: The metal sulfide is a chalcophile or siderophile element sulfide.

3. The method for preparing a hydrogen reduction lattice sulfur activation and regeneration metal sulfide mercury adsorbent according to claim 2, characterized in that: The metal sulfide is at least one of copper sulfide, zinc sulfide, molybdenum sulfide and cobalt sulfide.

4. The method for preparing a hydrogen reduction lattice sulfur activation and regeneration metal sulfide mercury adsorbent according to claim 1, characterized in that: The hydrogen concentration used in the adsorbent regeneration process ranges from 10 to 5000 ppm, and the reaction temperature is 100 to 600°C.

5. The method for preparing a hydrogen reduction lattice sulfur activation and regeneration metal sulfide mercury adsorbent according to claim 1, characterized in that: The hydrogen concentration used in the adsorbent reactivation process ranges from 10 to 5000 ppm and the reaction temperature is 100 to 600°C.

6. An apparatus for implementing the method for preparing a metal sulfide mercury adsorbent for activation and regeneration of lattice sulfur by hydrogen reduction according to any one of claims 1 to 5, characterized in that: The equipment includes two adsorption furnaces and a six-way valve, the two adsorption furnaces are respectively adsorption furnace I and adsorption furnace II, the six-way valve is provided with air inlet valve I, air inlet valve II, air inlet valve IV, air inlet valve V and air outlet valve III, air outlet valve VI, the adsorption furnace I is arranged on the pipeline connected between air outlet valve VI and air inlet valve V, the pipeline between the adsorption furnace I and the air inlet valve V is also provided with a three-way valve VII, the adsorption furnace II is arranged on the pipeline connected between air outlet valve III and air inlet valve IV, the pipeline between the adsorption furnace II and the air inlet valve IV is also provided with a three-way valve VIII.

7. The device for implementing the method for preparing a metal sulfide mercury adsorbent by hydrogen reduction lattice sulfur activation and regeneration according to claim 6, characterized in that: In the mercury adsorption process, the air inlet valve II is opened to introduce sulfur-containing mercury flue gas, and then the air outlet valve VI, the three-way valve VII, the air inlet valve V, and the air outlet valve III are opened in sequence. The sulfur-containing mercury flue gas flows along the route of air inlet valve II→air outlet valve VI→three-way valve VII→air inlet valve V→air outlet valve III, and passes through adsorption furnace I and adsorption furnace II in sequence, so that the mercury in the flue gas is captured by the mercury adsorbent in the adsorption furnace.

8. The device for implementing the method for preparing a metal sulfide mercury adsorbent by hydrogen reduction lattice sulfur activation and regeneration according to claim 6, characterized in that: During the adsorbent regeneration process, the air inlet valve I is opened to introduce hydrogen, and the air outlet valve VI is opened to allow hydrogen to pass through the adsorption furnace I, thereby increasing the furnace temperature to desorb and regenerate the adsorbent.

9. The device for implementing the method for preparing a metal sulfide mercury adsorbent by hydrogen reduction lattice sulfur activation and regeneration according to claim 6, characterized in that: During the adsorbent reactivation process, the air inlet valve I and the air inlet valve II are opened to introduce hydrogen and sulfur-containing mercury flue gas, and the air outlet valve VI, the three-way valve VII, the air inlet valve V and the air outlet valve III are opened to allow the air flow to flow along the route of air inlet valve II→air outlet valve VI→three-way valve VII→air inlet valve V→air outlet valve III. The hydrogen and the sulfur-containing mercury flue gas pass through the adsorption furnace I and the adsorption furnace II in turn to perform reverse disproportionation in situ reactivation on the adsorbent.

Citation Information

Patent Citations

  • Bromine loaded and sulfur rich activated carbon flue gas demercuration adsorbent and preparation method thereof

    CN107051391A

  • Preparation method of carbon-based sulfur-loaded iron-containing mercury removal adsorbent

    CN109499533A

  • Renewable composite gaseous zero-valent mercury adsorbent and preparation method thereof

    CN112316888A

  • High-sulfur high-humidity flue gas mercury removal self-sustaining activation adsorbent and preparation and regeneration method thereof

    CN115400719A

  • Method for recovering mercury adsorbent

    JP1992247237A

Cited By

  • Iron-activated sulfide, preparation method thereof and mercury trapping method

    CN121847058A