Fe2O3-In2O3 / Sn x Zr 1-x O2 composite oxygen carrier and its preparation method and application
By preparing Fe2O3-In2O3/SnxZr1-xO2 composite oxygen carrier, the problems of high cost, low efficiency and inability to recycle the catalyst in the prior art are solved, and efficient formaldehyde decomposition and catalytic performance are achieved.
Patent Information
- Application Number
- CN202411215394.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-02
AI Technical Summary
In the prior art, formaldehyde removal methods have problems such as high cost, low efficiency, low catalyst activity and inability to recycle, especially in the use of photocatalytic oxidation methods and precious metal catalysts.
The Fe2O3-In2O3/SnxZr1-xO2 composite oxygen carrier is prepared by adjusting the pH, precipitation and calcining steps to improve the mechanical properties and active sites of the oxygen carrier, and is used for the oxidative decomposition of formaldehyde.
It achieves high conversion rate formaldehyde decomposition, excellent catalytic performance and recyclable, reducing production costs and environmental impact.
Smart Images

Figure CN118719076B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of preparation and application of oxygen carriers, and specifically relates to Fe2O3-In2O3 / Sn x Zr 1-x O2 composite oxygen carrier and its preparation method and application. Background Art
[0002] Formaldehyde is a common indoor pollutant, often derived from building decoration, furniture and personal care products. Long-term low-concentration exposure can damage the human nervous system and respiratory system, and even cause cancer and gene mutations. The removal of formaldehyde is a difficult problem that must be faced in human health. Formaldehyde will only volatilize at high temperatures and is not easy to decompose. Common methods for removing formaldehyde include ventilation, adsorption, thermal catalytic oxidation and photocatalytic oxidation. However, the more thorough and effective way to remove formaldehyde is to decompose it, especially the catalytic oxidation method, which has a better effect. However, the photocatalytic oxidation method must be under ultraviolet irradiation to work, and the activity and efficiency of such catalysts are low. The use of precious metal catalysts is more expensive and the catalyst preparation is more complicated. The use of non-precious metal catalysts has a greater impact on the catalytic efficiency due to environmental conditions.
[0003] Composite oxygen carriers play an important role in chemical looping combustion technology. The conversion of fuel chemical energy into thermal energy is achieved by circulating the oxygen carrier between the oxidation and reduction reaction stages. As a carrier of oxygen, the composite oxygen carrier can be oxidized in the oxidation reactor and then react with the fuel in the reduction reactor to release heat. In this process, the composite oxygen carrier not only improves the combustion efficiency, but also significantly reduces pollutant emissions such as nitrogen oxides and sulfur dioxide. Composite oxygen carriers also play an important role in CO2 hydrogenation to olefins (Fe-based composite oxygen carriers, such as Fe / ZrO2, Fe / CeO2, Fe / TiO2, etc.) and methane reforming reactions (such as loading Ni on suitable carriers La2O3, CeO2 and Al2O3).
[0004] At present, composite oxygen carriers are mainly prepared by the sol-gel method and the chemical impregnation method. However, the mechanical strength of the composite oxygen carrier prepared by the sol-gel method is low, and the active components of the composite oxygen carrier prepared by the chemical impregnation method are unevenly distributed, both of which seriously affect its catalytic performance.
[0005] CN108579741A discloses a formaldehyde room temperature oxidation composite carrier catalyst prepared by sol-gel-impregnation method, the catalyst is composed of a granular carrier, titanium dioxide impregnated on the granular carrier, and a metal active component, wherein the metal active component is a noble metal (Pt, Pd, Au) or a mixture of a noble metal and an alkali metal (K or Na), and the titanium dioxide composite carrier is used as a carrier, which can completely catalytically oxidize high-concentration formaldehyde into CO2 and H2O. The catalyst of this method uses noble metal Pt and the like, which has a high cost, and the catalyst cannot be recycled, resulting in serious waste.
[0006] CN104694206A discloses an iron-based composite oxygen carrier and a preparation method thereof. The iron-based composite oxygen carrier comprises the following chemical components in mass fractions: Fe2O3 is 60-70, Al2O3 is 25-30, NiO is 5-10, and K2CO3 is 0-10; and is prepared by a sol-gel method, is suitable for a combined synergistic process of biomass chemical chain hydrogen production and tar production inhibition, and has the characteristics of high gasification efficiency and effective tar removal. The prepared oxygen carrier adopts the sol-gel method, and the preparation process is relatively complicated. At the same time, during the preparation of the oxygen carrier, the organic matter added has high requirements on the temperature control range, and the catalyst cannot be recycled. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a Fe2O3-In2O3 / Sn x Zr 1-x O2 composite oxygen carrier, strong mechanical properties, multiple active sites; the present invention also provides Fe2O3-In2O3 / Sn x Zr 1-x The preparation method of O2 composite oxygen carrier is simple to operate, pollution-free and industrializable; the Fe2O3-In2O3 / Sn x Zr 1-x O2 composite oxygen carrier is used for formaldehyde oxidation, with high decomposition conversion rate.
[0008] The Fe2O3-In2O3 / Sn x Zr 1-x The preparation method of O2 composite oxygen carrier comprises the following steps:
[0009] (1) Dissolve SnCl4·5H2O and ZrO(NO3)2·2H2O in water respectively, then mix and stir the two solutions for 30-60 min, adjust the pH value of the solution to 7-9, stir, filter, wash, dry, and calcine to obtain Sn x Zr 1-x O2;
[0010] (2) Sn xZr 1-x O2 is dissolved in water, Fe(NO3)3·9H2O and In(NO3)3·3H2O are added, a precipitant is added, stirred, precipitated at room temperature, filtered, washed, and dried;
[0011] (3) Grind the dried powder to a particle size range of 100-500 μm and calcine to obtain Fe2O3-In2O3 / Sn x Zr 1-x O2 composite oxygen carrier.
[0012] In step (1), pH is adjusted by using ammonia water, sodium hydroxide or potassium hydroxide solution with a mass concentration of 25-35%.
[0013] Step (1) After adjusting the pH value of the solution to 7-9, stirring at 80-120° C. for 8-12 hours, drying at 100-150° C. for 10-24 hours.
[0014] The precipitant in step (2) is thiourea or urea, and the Sn in step (2) x Zr 1-x The mass ratio of O2 to precipitant is (5-20):1.
[0015] Sn in step (2) x Zr 1-x The mass ratio of O2, Fe(NO3)3·9H2O, and In(NO3)3·3H2O is (1:3:2)-(7:5:5).
[0016] In step (2), the stirring temperature is 80-100° C., the stirring time is 8-12 h, the precipitation is carried out at room temperature for 10-15 h, the drying temperature is 80-100° C., and the drying time is 10-15 h.
[0017] The calcination in step (1) is carried out in a tubular furnace at a calcination temperature of 550-750° C., the calcination atmosphere is one of N2, H2, Ar, and He, and the calcination time is 5-10 hours; the calcination in step (3) is carried out in a tubular furnace at a calcination temperature of 550-850° C., the calcination atmosphere is one of N2, H2, Ar, and He, and the calcination time is 5-10 hours.
[0018] The Fe2O3-In2O3 / Sn x Zr 1-x In the O2 composite oxygen carrier, x is 0.2, 0.4, 0.6, and 0.8.
[0019] A Fe2O3-In2O3 / Sn x Zr 1-x The O2 composite oxygen carrier is composed of the Fe2O3-In2O3 / Sn x Zr 1-xThe invention is prepared by the preparation method of O2 composite oxygen carrier.
[0020] The Fe2O3-In2O3 / Sn x Zr 1-x The application of O2 composite oxygen carrier includes the following steps:
[0021] (1) Fe2O3-In2O3 / Sn x Zr 1-x Add O2 composite oxygen carrier into the fixed bed reactor, pre-treat with nitrogen at a flow rate of 100-500mL / min for 30-60min (exhaust the air and water vapor in the reactor), set the temperature of the preheater and the fixed bed reactor, the preheater is set at 200-400℃, the fixed bed reactor is set at 400-700℃, heat up, and set the reaction pressure to 0.3-1MPa (although pressurization is not conducive to formaldehyde decomposition, it is to improve mass transfer and reaction rate);
[0022] (2) introducing formaldehyde, setting the formaldehyde inlet flow rate to 50-100 mL / min, and obtaining gas phase products CO2 and H2O;
[0023] (3) After the reaction is completed, nitrogen is introduced to exhaust the air in the reactor, and oxygen is continued to be introduced into the fixed bed. The temperature of the fixed bed reactor is set at 400-600°C to obtain Fe2O3-In2O3 / Sn with restored lattice oxygen. x Zr 1-x O2 composite oxygen carrier.
[0024] Specifically, the Fe2O3-In2O3 / Sn x Zr 1-x The preparation method of O2 (x is 0.2, 0.4, 0.6, 0.8) composite oxygen carrier comprises the following steps:
[0025] (1) Dissolve SnCl4·5H2O and ZrO(NO3)2·2H2O in water respectively, then mix and stir the two solutions for 30-60 min, adjust the pH value to 7-9 with 25-35% ammonia water, sodium hydroxide or potassium hydroxide solution, stir at 80-120℃ for 8-12h, filter and wash with deionized water to remove impurity ions, dry at 100-150℃ for 10-24h, and calcine at 550-750℃ for 5-10h in a tube furnace in N2 / H2 / Ar / He atmosphere to obtain Sn x Zr 1-x O2.
[0026] (2) Sn x Zr 1-xO2 is dissolved in water, Fe(NO3)3·9H2O and In(NO3)3·3H2O are added, thiourea or urea as a precipitant is added, stirred at 80-100℃ for 8-12h, precipitated at room temperature for 10-15h, filtered and washed, and dried at 80-100℃ for 10-15h; Sn x Zr 1-x The mass ratio of O2 to precipitant is (5-20):1, Sn x Zr 1-x The mass ratio of O2, Fe(NO3)3·9H2O, and In(NO3)3·3H2O is (1:3:2)-(7:5:5).
[0027] (3) The dried powder was ground into a particle size range of 100-500 μm and calcined in a tube furnace at 550-850 °C for 5-10 h in an atmosphere of N2 / H2 / Ar / He to obtain Fe2O3-In2O3 / Sn x Zr 1-x O2 composite oxygen carrier.
[0028] The present invention provides Fe2O3-In2O3 / Sn x Zr 1-x The preparation method of O2 composite oxygen carrier, due to the doping of zirconium in the tin oxide framework, increases the specific surface area of the oxygen carrier, increases the oxygen vacancies, and also increases the content of lattice oxygen in the oxygen carrier, thereby promoting the oxidative decomposition of formaldehyde. The prepared composite oxygen carrier has a large specific surface area, many oxygen vacancies, and rich lattice oxygen content. The composite oxygen carrier is used to decompose formaldehyde to produce CO2 and H2O.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) Fe2O3-In2O3 / Sn prepared by the method of the present invention x Zr 1-x Compared with the traditional single oxygen carrier, the O2 composite oxygen carrier of the present invention is a composite carrier composed of two oxides, which is beneficial to the prepared composite oxygen carrier with large specific surface area, more oxygen vacancies and rich lattice oxygen content.
[0031] (2) Fe2O3-In2O3 / Sn prepared by the present invention x Zr 1-x O2 composite oxygen carrier, when used for formaldehyde decomposition, has high conversion rate and simple regeneration operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Fe2O3-In2O3 / Sn prepared in Example 1 x Zr 1-x TEM image of O2 composite oxygen carrier.
[0033] Figure 2 Fe2O3-In2O3 / Sn prepared in Example 1 x Zr 1-x TEM image of O2 composite oxygen carrier after 10 cycles of formaldehyde decomposition. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with specific embodiments.
[0035] The raw materials and reagents used in the following examples and comparative examples are all commercially available products. The operations of adding water and dissolving described below are all for creating a reaction environment and do not participate in the reaction. They only need to ensure that the reaction proceeds completely and are not further limited.
[0036] Example 1
[0037] The Fe2O3-In2O3 / Sn 0.2 Zr 0.8 The preparation method of O2 composite oxygen carrier comprises the following steps:
[0038] (1) SnCl4·5H2O and ZrO(NO3)2·2H2O were reacted according to the product Sn 0.2 Zr 0.8 O2 ingredients were dissolved in water respectively, and then the two solutions were mixed and stirred for 40 minutes, and the pH value was adjusted to 8 with a 30% ammonia solution, stirred at 100℃ for 9 hours, filtered, washed with deionized water, dried at 120℃ for 12 hours, and calcined at 650℃ for 6 hours in a tube furnace with N2 atmosphere to obtain Sn 0.2 Zr 0.8 O2.
[0039] (2) According to Sn 0.2 Zr 0.8 The mass ratio of O2, Fe(NO3)3·9H2O and In(NO3)3·3H2O is 1:3:2. 0.2 Zr 0.8 O2 is dissolved in water, Fe(NO3)3·9H2O and In(NO3)3·3H2O are added, and Sn 0.2 Zr 0.8 The mass ratio of O2 to thiourea is 10:1. Add thiourea as precipitant, stir at 90℃ for 9h, precipitate at room temperature for 12h, filter and wash, and dry at 90℃ for 12h.
[0040] (3) The dried powder was ground into a particle size range of 100-500 μm and calcined in a tube furnace at 680 °C for 8 h in a N2 atmosphere to obtain Fe2O3-In2O3 / Sn 0.2 Zr 0.8O2 composite oxygen carrier, its TEM image is as follows Figure 1 shown.
[0041] The Fe2O3-In2O3 / Sn 0.2 Zr 0.8 O2 composite oxygen carrier is used for formaldehyde decomposition, including the following steps:
[0042] (1) Fe2O3-In2O3 / Sn 0.2 Zr 0.8 O2 composite oxygen carrier was added to the fixed bed reactor, and nitrogen was passed through the reactor for pretreatment at a flow rate of 400 mL / min for 40 min. The preheater temperature was set at 300 °C, the fixed bed reactor reaction temperature was set at 500 °C, and the temperature was increased. The reaction pressure was set at 0.6 MPa.
[0043] (2) Formaldehyde was introduced, and the formaldehyde inlet flow rate was set to 100 mL / min to obtain gas phase products CO2 and H2O;
[0044] (3) After the reaction is completed, nitrogen is introduced to exhaust the air in the reactor, and oxygen is continued to be introduced into the fixed bed. The temperature of the fixed bed reactor is set at 500°C to obtain Fe2O3-In2O3 / Sn with restored lattice oxygen. 0.2 Zr 0.8 O2 composite oxygen carrier. The Fe2O3-In2O3 / Sn after the lattice oxygen is restored 0.2 Zr 0.8 The O2 composite oxygen carrier was used for the above formaldehyde decomposition and cycled 10 times to calculate the formaldehyde conversion rate. 0.2 Zr 0.8 TEM image of O2 composite oxygen carrier Figure 2 shown.
[0045] Example 2
[0046] The Fe2O3-In2O3 / Sn 0.4 Zr 0.6 The preparation method of O2 composite oxygen carrier comprises the following steps:
[0047] (1) SnCl4·5H2O and ZrO(NO3)2·2H2O were reacted according to the product Sn 0.4 Zr 0.6 O2 ingredients were dissolved in water respectively, and then the two solutions were mixed and stirred for 30 minutes, and the pH value was adjusted to 7 with a sodium hydroxide solution with a mass concentration of 35%, stirred at 80℃ for 12 hours, filtered and washed with deionized water, dried at 150℃ for 10 hours, and calcined at 550℃ for 10 hours in a tube furnace with H2 atmosphere to obtain Sn 0.4 Zr 0.6O2.
[0048] (2) According to Sn 0.4 Zr 0.6 The mass ratio of O2, Fe(NO3)3·9H2O and In(NO3)3·3H2O is 3:5:2. 0.4 Zr 0.6 O2 is dissolved in water, Fe(NO3)3·9H2O and In(NO3)3·3H2O are added, and Sn 0.2 Zr 0.8 The mass ratio of O2 to thiourea is 20:1. Add thiourea as precipitant, stir at 100℃ for 8h, precipitate at room temperature for 15h, filter and wash, and dry at 100℃ for 10h.
[0049] (3) The dried powder was ground into a particle size range of 100-500 μm and calcined in a tube furnace at 750 °C for 6 h in a H2 atmosphere to obtain Fe2O3-In2O3 / Sn 0.4 Zr 0.6 O2 composite oxygen carrier.
[0050] The Fe2O3-In2O3 / Sn 0.4 Zr 0.6 O2 composite oxygen carrier is used for formaldehyde decomposition, including the following steps:
[0051] (1) Fe2O3-In2O3 / Sn 0.4 Zr 0.6 O2 composite oxygen carrier was added to the fixed bed reactor, and nitrogen was passed through the reactor for pretreatment at a flow rate of 100 mL / min for 60 min. The preheater was set at 400 °C, the fixed bed reactor was set at 700 °C, and the temperature was increased. The reaction pressure was set to 0.3 MPa.
[0052] (2) Formaldehyde was introduced, and the formaldehyde inlet flow rate was set to 100 mL / min to obtain gas phase products CO2 and H2O;
[0053] (3) After the reaction is completed, nitrogen is introduced to exhaust the air in the reactor, and oxygen is continued to be introduced into the fixed bed. The temperature of the fixed bed reactor is set at 600°C to obtain Fe2O3-In2O3 / Sn with restored lattice oxygen. 0.4 Zr 0.6 O2 composite oxygen carrier, continue to apply.
[0054] Example 3
[0055] The Fe2O3-In2O3 / Sn 0.6 Zr 0.4 The preparation method of O2 composite oxygen carrier comprises the following steps:
[0056] (1) SnCl4·5H2O and ZrO(NO3)2·2H2O were reacted according to the product Sn 0.6 Zr 0.4 O2 ingredients were dissolved in water respectively, and then the two solutions were mixed and stirred for 30 minutes, and the pH value was adjusted to 9 with a potassium hydroxide solution with a mass concentration of 25%, stirred at 80℃ for 12 hours, filtered and washed with deionized water, dried at 100℃ for 24 hours, and calcined at 750℃ in an Ar atmosphere in a tube furnace for 5 hours to obtain Sn 0.6 Zr 0.4 O2.
[0057] (2) According to Sn 0.6 Zr 0.4 O2, Fe(NO3)3·9H2O, In(NO3)3·3H2O were prepared in a mass ratio of 6:7:3. 0.6 Zr 0.4 O2 is dissolved in water, Fe(NO3)3·9H2O and In(NO3)3·3H2O are added, and Sn 0.6 Zr 0.4 The mass ratio of O2 to urea is 20:1. Add urea as a precipitant, stir at 80°C for 12 hours, precipitate at room temperature for 10 hours, filter and wash, and dry at 80°C for 15 hours.
[0058] (3) The dried powder was ground into a particle size range of 100-500 μm and calcined in a tube furnace at 850 °C for 5 h in an Ar atmosphere to obtain Fe2O3-In2O3 / Sn 0.6 Zr 0.4 O2 composite oxygen carrier.
[0059] The Fe2O3-In2O3 / Sn 0.6 Zr 0.4 O2 composite oxygen carrier is used for formaldehyde decomposition, including the following steps:
[0060] (1) Fe2O3-In2O3 / Sn 0.6 Zr 0.4 O2 composite oxygen carrier was added to the fixed bed reactor, and nitrogen was passed through the reactor for pretreatment at a flow rate of 500 mL / min for 60 min. The preheater was set at 200 °C, the fixed bed reactor was set at 400 °C, and the temperature was increased. The reaction pressure was set at 0.8 MPa.
[0061] (2) Formaldehyde was introduced, and the formaldehyde inlet flow rate was set to 50 mL / min to obtain gas phase products CO2 and H2O;
[0062] (3) After the reaction is completed, nitrogen is introduced to exhaust the air in the reactor, and oxygen is continued to be introduced into the fixed bed. The temperature of the fixed bed reactor is set at 400°C to obtain Fe2O3-In2O3 / Sn with restored lattice oxygen. 0.6 Zr 0.4 O2 composite oxygen carrier, continue to apply.
[0063] Example 4
[0064] The Fe2O3-In2O3 / Sn 0.8 Zr 0.2 The preparation method of O2 composite oxygen carrier comprises the following steps:
[0065] (1) SnCl4·5H2O and ZrO(NO3)2·2H2O were reacted according to the product Sn 0.8 Zr 0.2 O2 ingredients were dissolved in water respectively, and then the two solutions were mixed and stirred for 60 minutes, and the pH value was adjusted to 8 with a 30% ammonia solution, stirred at 120℃ for 8 hours, filtered and washed with deionized water, dried at 110℃ for 11 hours, and calcined at 650℃ in a tube furnace with He atmosphere for 6 hours to obtain Sn 0.8 Zr 0.2 O2.
[0066] (2) According to Sn 0.8 Zr 0.2 O2, Fe(NO3)3·9H2O, In(NO3)3·3H2O were prepared in a mass ratio of 7:5:5. 0.8 Zr 0.2 O2 is dissolved in water, Fe(NO3)3·9H2O and In(NO3)3·3H2O are added, and Sn 0.6 Zr 0.4 The mass ratio of O2 to urea is 10:1. Add urea as a precipitant, stir at 90°C for 10 hours, precipitate at room temperature for 12 hours, filter and wash, and dry at 90°C for 12 hours.
[0067] (3) The dried powder was ground into a particle size range of 100-500 μm and calcined in a tube furnace at 750 °C for 7 h in a He atmosphere to obtain Fe2O3-In2O3 / Sn 0.8 Zr 0.2 O2 composite oxygen carrier.
[0068] The Fe2O3-In2O3 / Sn 0.8 Zr 0.2 O2 composite oxygen carrier is used for formaldehyde decomposition, including the following steps:
[0069] (1) Fe2O3-In2O3 / Sn 0.8 Zr0.2 O2 composite oxygen carrier was added to the fixed bed reactor, and nitrogen was passed through the reactor for pretreatment at a flow rate of 300 mL / min for 40 min. The preheater was set at 300 °C, the fixed bed reactor was set at a reaction temperature of 500 °C, and the temperature was increased and the reaction pressure was set at 1 MPa.
[0070] (2) Formaldehyde was introduced, and the formaldehyde inlet flow rate was set to 100 mL / min to obtain gas phase products CO2 and H2O;
[0071] (3) After the reaction is completed, nitrogen is introduced to exhaust the air in the reactor, and oxygen is continued to be introduced into the fixed bed. The temperature of the fixed bed reactor is set at 600°C to obtain Fe2O3-In2O3 / Sn with restored lattice oxygen. 0.8 Zr 0.2 O2 composite oxygen carrier, continue to apply.
[0072] Comparative Example 1
[0073] A method for preparing a Fe2O3-In2O3 / ZrO2 oxygen carrier comprises the following steps:
[0074] (1) ZrO(NO3)2·2H2O was dissolved in water and then stirred for 40 min. The pH value was adjusted to 8 with 30% ammonia solution, stirred at 100°C for 9 h, filtered, washed with deionized water, dried at 120°C for 12 h, and calcined at 650°C in a tube furnace in N2 atmosphere for 6 h to obtain ZrO2.
[0075] (2) Prepare ZrO2, Fe(NO3)3·9H2O and In(NO3)3·3H2O in a mass ratio of 1:3:2. Dissolve ZrO2 in water, add Fe(NO3)3·9H2O and In(NO3)3·3H2O, add precipitant thiourea in a mass ratio of ZrO2 to thiourea of 10:1, stir at 90°C for 9 h, precipitate at room temperature for 12 h, filter and wash, and dry at 90°C for 12 h.
[0076] (3) The dried powder was ground into a particle size range of 100-500 μm and calcined in a tube furnace at 680° C. for 8 h in a N 2 atmosphere to obtain a Fe 2 O 3 -In 2 O 3 / ZrO 2 oxygen carrier.
[0077] The Fe2O3-In2O3 / ZrO2 oxygen carrier prepared above is used for formaldehyde decomposition, comprising the following steps:
[0078] (1) Fe2O3-In2O3 / ZrO2 oxygen carrier was added to a fixed bed reactor, and nitrogen was passed through the reactor for pretreatment at a flow rate of 400 mL / min for 40 min. The preheater temperature was set at 300 °C, the fixed bed reactor reaction temperature was set at 500 °C, and the temperature was increased. The reaction pressure was set to 0.6 MPa.
[0079] (2) Formaldehyde was introduced, and the formaldehyde inlet flow rate was set to 100 mL / min to obtain gas phase products CO2 and H2O;
[0080] (3) After the reaction is completed, nitrogen is introduced to exhaust the air in the reactor, and oxygen is continued to be introduced into the fixed bed. The temperature of the fixed bed reactor is set at 500°C to obtain Fe2O3-In2O3 / ZrO2 oxygen carrier.
[0081] Comparative Example 2
[0082] A method for preparing a Fe2O3-In2O3 / SnO2 oxygen carrier comprises the following steps:
[0083] (1) Dissolve SnCl4·5H2O in water and stir for 40 min. Adjust the pH value to 8 with 30% ammonia solution. Stir at 100°C for 9 h. Filter, wash with deionized water, dry at 120°C for 12 h, and calcine at 650°C in a tube furnace under N2 atmosphere for 6 h to obtain SnO2.
[0084] (2) Prepare SnO2, Fe(NO3)3·9H2O and In(NO3)3·3H2O in a mass ratio of 1:3:2. Dissolve SnO2 in water, add Fe(NO3)3·9H2O and In(NO3)3·3H2O, add precipitant thiourea in a mass ratio of SnO2 to thiourea of 10:1, stir at 90°C for 9 h, precipitate at room temperature for 12 h, filter and wash, and dry at 90°C for 12 h.
[0085] (3) The dried powder was ground into a particle size range of 100-500 μm and calcined in a tube furnace at 680° C. for 8 h in a N 2 atmosphere to obtain a Fe 2 O 3 -In 2 O 3 / SnO 2 oxygen carrier.
[0086] The Fe2O3-In2O3 / SnO2 oxygen carrier prepared above is used for formaldehyde decomposition, comprising the following steps:
[0087] (1) Fe2O3-In2O3 / SnO2 oxygen carrier was added to a fixed bed reactor, and nitrogen was passed through the reactor for pretreatment at a flow rate of 400 mL / min for 40 min. The preheater temperature was set at 300 °C, the fixed bed reactor reaction temperature was set at 500 °C, and the temperature was increased. The reaction pressure was set to 0.6 MPa.
[0088] (2) Formaldehyde is introduced, and the formaldehyde inlet flow rate is set to 10 mL / min to obtain gas phase products CO2 and H2O;
[0089] (3) After the reaction is completed, nitrogen is introduced to exhaust the air in the reactor, and oxygen is continued to be introduced into the fixed bed. The temperature of the fixed bed reactor is set at 500°C to obtain a Fe2O3-In2O3 / SnO2 oxygen carrier with restored lattice oxygen.
[0090] Comparative Example 3
[0091] A method for preparing a Fe2O3-In2O3 oxygen carrier comprises the following steps:
[0092] (1) Prepare the mixture according to the mass ratio of Fe(NO3)3·9H2O and In(NO3)3·3H2O of 3:2. Dissolve Fe(NO3)3·9H2O and In(NO3)3·3H2O in water, add 20 mg of precipitant thiourea, stir at 90°C for 9 h, precipitate at room temperature for 12 h, filter and wash, and dry at 90°C for 12 h.
[0093] (2) The dried powder was ground into a particle size range of 100-500 μm and calcined in a tube furnace at 680° C. for 8 h in a N 2 atmosphere to obtain a Fe 2 O 3 -In 2 O 3 oxygen carrier.
[0094] The Fe2O3-In2O3 oxygen carrier prepared above is used for formaldehyde decomposition, comprising the following steps:
[0095] (1) Fe2O3-In2O3 oxygen carrier was added to a fixed bed reactor, and nitrogen was passed through the reactor for pretreatment at a flow rate of 400 mL / min for 40 min. The preheater temperature was set at 300 °C, the fixed bed reactor reaction temperature was set at 500 °C, and the temperature was increased. The reaction pressure was set to 0.6 MPa.
[0096] (2) Formaldehyde was introduced, and the formaldehyde inlet flow rate was set to 100 mL / min to obtain gas phase products CO2 and H2O;
[0097] (3) After the reaction is completed, nitrogen is introduced to exhaust the air in the reactor, and oxygen is continued to be introduced into the fixed bed. The temperature of the fixed bed reactor is set at 500°C to obtain a Fe2O3-In2O3 oxygen carrier with restored lattice oxygen.
[0098] The oxygen carriers prepared in the above examples and comparative examples were tested for performance, and the test results are shown in Table 1. After the prepared oxygen carriers were applied to formaldehyde decomposition, the formaldehyde conversion rate and CO2 yield were shown in Table 2. After the oxygen carrier prepared in Example 1 was cyclically degraded for 10 times, the formaldehyde conversion rate and CO2 yield were shown in Table 3.
[0099] The calculation formula of formaldehyde conversion rate is:
[0100] ;
[0101] η is the conversion rate of formaldehyde, M HCHO,in and M HCHO,out They are the formaldehyde intake and formaldehyde output respectively.
[0102] χ is the CO2 production rate, M CO2,out is the output of CO2.
[0103] Table 1 Test results
[0104]
[0105] Table 2 Oxygen carriers for formaldehyde decomposition results
[0106]
[0107] Table 3 Experimental results of Example 1 repeated 10 times
[0108]
[0109] It can be seen from Table 1 that the average bulk density, average specific surface area, average pore volume, and average pore size of the composite oxygen carrier prepared by the present invention are relatively large, the crushing strength is relatively large, and the catalytic performance of the composite oxygen carrier prepared by the present invention is good. It can be seen from Table 2 that when the composite oxygen carrier prepared by the present invention is used for the decomposition of HCHO, the decomposition conversion rate is high and the oxidation decomposition performance is strong. Figure 2 It can be seen that the composite oxygen carrier prepared by the present invention can be recycled, and the catalytic performance of the recycled composite oxygen carrier is still good.
Claims
1. Fe2O3-In2O3 / Sn x Zr 1-x The preparation method of O2 composite oxygen carrier is characterized by: The following steps are involved: (1) Dissolve SnCl4·5H2O and ZrO(NO3)2·2H2O in water respectively, then mix and stir the two solutions for 30-60 min, adjust the pH value of the solution to 7-9, stir, filter, wash, dry, and calcine to obtain Sn x Zr 1-x O2; where x is 0.2, 0.4, 0.6, 0.8; (2) Sn x Zr 1-x O2 is dissolved in water, Fe(NO3)3·9H2O and In(NO3)3·3H2O are added, a precipitant is added, stirred, precipitated at room temperature, filtered, washed, and dried; (3) Grind the dried powder to a particle size range of 100-500 μm and calcine to obtain Fe2O3-In2O3 / Sn x Zr 1-x O2 composite oxygen carrier.
2. Fe2O3-In2O3 / Sn according to claim 1 x Zr 1-x The preparation method of O2 composite oxygen carrier is characterized by: In step (1), pH is adjusted by using ammonia water, sodium hydroxide or potassium hydroxide solution with a mass concentration of 25-35%.
3. Fe2O3-In2O3 / Sn according to claim 1 x Zr 1-x The preparation method of O2 composite oxygen carrier is characterized by: Step (1) After adjusting the pH value of the solution to 7-9, stirring at 80-120° C. for 8-12 hours, drying at 100-150° C. for 10-24 hours.
4. Fe2O3-In2O3 / Sn according to claim 1 x Zr 1-x The preparation method of O2 composite oxygen carrier is characterized by: The precipitant in step (2) is thiourea or urea, and the Sn in step (2) x Zr 1-x The mass ratio of O2 to precipitant is (5-20):
1.
5. Fe2O3-In2O3 / Sn according to claim 1 x Zr 1-x The preparation method of O2 composite oxygen carrier is characterized by: Sn in step (2) x Zr 1-x The mass ratio of O2, Fe(NO3)3·9H2O, and In(NO3)3·3H2O is 1:3:2, 3:5:2, 6:7:3 or 7:5:
5.
6. Fe2O3-In2O3 / Sn according to claim 1 x Zr 1-x The preparation method of O2 composite oxygen carrier is characterized by: In step (2), the stirring temperature is 80-100° C., the stirring time is 8-12 h, the precipitation is carried out at room temperature for 10-15 h, the drying temperature is 80-100° C., and the drying time is 10-15 h.
7. Fe2O3-In2O3 / Sn according to claim 1 x Zr 1-x The preparation method of O2 composite oxygen carrier is characterized by: The calcination in step (1) is carried out in a tubular furnace at a calcination temperature of 550-750° C., the calcination atmosphere is one of N2, H2, Ar, and He, and the calcination time is 5-10 hours; the calcination in step (3) is carried out in a tubular furnace at a calcination temperature of 550-850° C., the calcination atmosphere is one of N2, H2, Ar, and He, and the calcination time is 5-10 hours.
8. A Fe2O3-In2O3 / Sn x Zr 1-x O2 composite oxygen carrier, characterized in that: The Fe2O3-In2O3 / Sn according to any one of claims 1 to 7 x Zr 1-x The invention is prepared by the preparation method of O2 composite oxygen carrier.
9. Fe2O3-In2O3 / Sn as claimed in claim 8 x Zr 1-x The application of O2 composite oxygen carrier is characterized by: The following steps are involved: (1) Fe2O3-In2O3 / Sn x Zr 1-x Add O2 composite oxygen carrier into the fixed bed reactor, pre-treat with nitrogen at a flow rate of 100-500mL / min for 30-60min, set the temperature of the preheater and the fixed bed reactor, the preheater is set at 200-400℃, the fixed bed reactor is set at 400-700℃, heat up, and set the reaction pressure to 0.3-1MPa; (2) introducing formaldehyde, setting the formaldehyde inlet flow rate to 50-100 mL / min, and obtaining gas phase products CO2 and H2O; (3) After the reaction is completed, nitrogen is introduced to exhaust the air in the reactor, and oxygen is continued to be introduced into the fixed bed. The temperature of the fixed bed reactor is set at 400-600°C to obtain Fe2O3-In2O3 / Sn with restored lattice oxygen. x Zr 1-x O2 composite oxygen carrier.