Iron oxide / bismuth ferrite heterojunction material and preparation method thereof
By controlling the molar ratio of bismuth and iron, alkali solution concentration and microwave hydrothermal reaction conditions, iron oxide/bismuth ferrite heterojunction materials were prepared, which solved the problem of low photocatalytic water oxidation efficiency of BiFeO3 materials and achieved efficient photocatalysis. performance.
Patent Information
- Application Number
- CN202410774284.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult for existing BiFeO3 materials to effectively separate and migrate photogenerated charges during photocatalytic water oxidation, and the catalytic efficiency is low.
By controlling the molar ratio of bismuth and iron, the concentration of the alkali solution and the microwave hydrothermal reaction conditions, the iron oxide/bismuth ferrite heterojunction material is prepared to achieve in-situ growth of iron oxide on the surface of bismuth ferrite, improving the interface quality and Catalytic efficiency.
The space-time separation efficiency of carriers is improved, the catalytic efficiency of the photocatalyst is significantly improved, and the oxygen production performance reaches 2 to 3 times that of the same type of materials.
Smart Images

Figure CN118719077A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of photocatalysts, and in particular to an iron oxide / bismuth ferrite heterojunction material and a method for preparing the material. Background Art
[0002] Bismuth ferrite (BiFeO3) is a typical ferroelectric material with a perovskite structure. It has a narrow bandgap and a significant photovoltaic effect in the visible light range and near the visible light range. In particular, its valence band top potential is more positive than that of O2 / H2O (1.23Vvs.NHE), so it has great potential in the field of photocatalytic water oxidation. However, the current BiFeO3 material has the disadvantages of being difficult to effectively separate and migrate photogenerated charges and having low catalytic efficiency. Summary of the invention
[0003] In view of this, the present application provides a method for preparing an iron oxide / bismuth ferrite heterojunction material, the preparation method comprising: mixing a bismuth source compound, an iron source compound and an acid solution, wherein the molar ratio of bismuth in the bismuth source compound to iron in the iron source compound is 1:2 to 1.5:1, to obtain a first mixed solution; providing an alkaline solution with a concentration of 2M to 8M, mixing the first mixed solution with the alkaline solution, so that the bismuth in the bismuth source compound and the iron in the iron source compound form bismuth hydroxide and iron hydroxide, respectively, to obtain a second mixed solution; using microwaves to assist the second mixed solution in a hydrothermal reaction, the hydrothermal reaction temperature is 140 to 180°C, and the time is 30 to 50 minutes, to obtain an intermediate product; washing and drying the intermediate product to obtain the iron oxide / bismuth ferrite heterojunction material.
[0004] In some possible implementations, the bismuth source compound is selected from one or more of bismuth nitrate and its hydrate, bismuth sulfate and its hydrate, and bismuth acetate and its hydrate.
[0005] In some possible implementations, the iron source compound is selected from one or more of ferric nitrate and its hydrates, ferric sulfate and its hydrates, and ferric acetate and its hydrates.
[0006] In some possible implementations, the acid solution includes nitric acid.
[0007] In some possible implementations, the temperature of the alkaline solution is 25-30°C.
[0008] In some possible implementations, the alkaline solution is selected from one of potassium hydroxide and sodium hydroxide.
[0009] In some possible implementations, after the first mixed solution and the alkaline solution are mixed, stirring is further performed, and the stirring time is 1 to 6 hours.
[0010] In some possible implementations, the drying temperature is 50 to 80° C., and the drying time is 6 to 24 hours.
[0011] The present application also provides an iron oxide / bismuth ferrite heterojunction material, which is prepared by the preparation method.
[0012] The present application controls the ratio of bismuth source compound and iron source compound, the concentration of alkaline solution, hydrothermal reaction temperature and reaction time, so that while synthesizing bismuth ferrite, iron oxide grows in situ on the surface of bismuth ferrite, realizing the construction of iron oxide / bismuth ferrite heterojunction; the present application also quickly heats up to the temperature required for material crystallization and growth through microwaves, and can obtain heterojunctions in a short time. Compared with the defects of the traditional hydrothermal method, which is long in time and low in safety factor, and the sol-gel method, which is long in process time and complicated in operation, the microwave-assisted hydrothermal reaction constructs the process of iron oxide / bismuth ferrite heterojunction quickly and efficiently, avoiding the disordered crystal growth and uneven size caused by uneven heating, saving time cost and economic investment, and reducing energy loss. The atoms at the interface of the obtained heterojunction form good contact, which is more conducive to promoting charge transfer, further improving the relevant properties of the composite material, and can be applied to photocatalytic hydrolysis oxygen production, organic pollutant degradation and organic synthesis as a photocatalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a transmission electron microscopy image of the iron oxide / bismuth ferrite heterogeneous material provided in Example 1 of the present application.
[0014] Figure 2 This is the X-ray diffraction pattern of the iron oxide / bismuth ferrite heterogeneous material provided in Example 1 of the present application.
[0015] Figure 3 This is the energy dispersive X-ray spectrum of the iron oxide / bismuth ferrite heterogeneous material provided in Example 1 of the present application.
[0016] Figure 4 X-ray diffraction patterns of the final products provided for Examples 1-3 and Comparative Examples 1-3 of the present application.
[0017] Figure 5 The oxygen production activity test results of the final products provided for Examples 1-3 and Comparative Examples 1-2 of the present application.
[0018] Figure 6 X-ray diffraction patterns of the final products provided for Example 1, Examples 4-5 and Comparative Examples 4-5 of the present application.
[0019] Figure 7 X-ray diffraction patterns of the final products provided for Example 1, Examples 6-7 and Comparative Examples 6-7 of the present application.
[0020] Figure 8 X-ray diffraction patterns of the final products provided for Example 1, Examples 8-9 and Comparative Examples 8-10 of the present application. DETAILED DESCRIPTION
[0021] The embodiments of the present application are described in detail below. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application; it should be noted that, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of the present application; in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other; many specific details are elaborated in the following description to facilitate a full understanding of the present application, and the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0022] The construction of heterojunctions by combining metal-semiconductors, semiconductor-semiconductors, etc. with matching Fermi levels or electronic structures, and utilizing the built-in electric field generated at the contact surface of different materials is considered to be one of the effective means to improve the separation efficiency of carriers, and it has been theoretically proven that high-quality interfaces can improve the time-space separation efficiency of carriers. However, most of the bismuth ferrite-based heterojunction materials reported so far are prepared by physical mixing methods, and the material interfaces are poor.
[0023] In view of this, an embodiment of the present application provides a method for preparing an iron oxide / bismuth ferrite heterojunction material, the preparation method comprising:
[0024] The first step: mixing a bismuth source compound, an iron source compound and an acid solution, wherein the molar ratio of bismuth in the bismuth source compound to iron in the iron source compound is 1:2 to 1.5:1, to obtain a first mixed solution.
[0025] On the one hand, the present application controls the molar ratio of bismuth to iron to be 1:2 to 1.5:1, so that during the subsequent growth of bismuth ferrite BiFeO3 crystals, the iron element can grow in situ on the surface of bismuth ferrite to form iron oxide (Fe2O3), improve the interface properties of BiFeO3 and iron oxide, and achieve the construction of high-quality iron oxide / bismuth ferrite heterojunction. The present application found that when the molar ratio of bismuth to iron is greater than 1.5:1, that is, when the bismuth content in the preparation system is too high, bismuth dominates the molecular collision and competition process, and the preparation system is more inclined to form a crystal form of Bi 25 FeO 40In the process of preparing bismuth ferrite, Fe2O3 is more inclined to participate in the formation of the crystal rather than grow independently in situ on the surface of bismuth ferrite. Moreover, when the bismuth content is too high, it may also cause the bismuth element to precipitate directly in the form of crystals. When the molar ratio of bismuth to iron is less than 1:2, that is, when the bismuth content in the preparation system is too low, it is difficult to form BiFeO3 with a complete crystal structure, resulting in a decrease in the separation efficiency of carriers. Therefore, controlling the molar ratio of bismuth to iron to 1:2 to 1.5:1, on the one hand, provides sufficient material basis for the formation of the BiFeO3 crystal structure, and on the other hand, it is beneficial to reduce the participation of the generated Fe2O3 in the BiFeO3 crystal structure. 25 FeO 40 The risks in the formation of crystalline bismuth ferrite were eliminated, thereby successfully constructing an iron oxide / bismuth ferrite heterojunction based on in-situ growth.
[0026] In some embodiments, the bismuth source compound is selected from one or more of bismuth nitrate and its hydrate, bismuth sulfate and its hydrate, and bismuth acetate and its hydrate; the iron source compound is selected from one or more of ferric nitrate and its hydrate, ferric sulfate and its hydrate, and ferric acetate and its hydrate.
[0027] In some embodiments, the acid solution comprises nitric acid.
[0028] Step 2: providing an alkaline solution with a concentration of 2M to 8M, mixing the first mixed solution with the alkaline solution, so that the bismuth in the bismuth source compound and the iron in the iron source compound form bismuth hydroxide and iron hydroxide respectively, to obtain a second mixed solution.
[0029] On the one hand, the present application also controls the concentration of the alkaline solution so that during the subsequent growth of bismuth ferrite BiFeO3 crystals, the iron element can in situ grow Fe2O3 on the surface of bismuth ferrite, further improving the interface quality of BiFeO3 and iron oxide, and realizing the construction of high-quality iron oxide / bismuth ferrite heterojunction. The present application has found that the concentration of the alkaline solution will affect the formation of the bismuth ferrite / iron oxide heterojunction. When the concentration of the alkaline solution is low, such as less than 1M, it is not conducive to the formation of Fe2O3. This is because, according to analysis, the alkaline solution acts as a mineralizer in the preparation process, which can improve the crystallinity of bismuth ferrite under short-term high temperature and high pressure conditions. As the concentration of the mineralizer increases, the probability of bismuth and iron combining to form a trigonal phase BiFeO3 in the preparation system increases; accordingly, the present application increases the concentration of the alkaline solution and finds that when the concentration reaches about 2M, the bismuth ferrite / iron oxide heterojunction begins to form, but when the concentration of the alkaline solution exceeds 8M, it is again not conducive to the formation of Fe2O3. It is speculated that at this time, the iron element tends to participate in the construction of other crystal forms of bismuth ferrite, rather than growing independently in situ on the BiFeO3 surface in the form of Fe2O3 crystals. Therefore, the present application controls the concentration of the alkaline solution within the range of 2M to 8M, which is conducive to the formation of Fe2O3 in the preparation system, thereby helping to construct an iron oxide / bismuth ferrite heterojunction based on in situ growth.
[0030] In some embodiments, the temperature of the alkaline solution is 25-30°C.
[0031] By adjusting the temperature of the alkaline solution mixed with the first mixed solution, it is beneficial to reduce the influence of the high temperature environment on the solubility of the bismuth source and the iron source in the preparation system, thereby accurately controlling the molar ratio of the bismuth source and the iron source when feeding, and further facilitating the formation of high-quality iron oxide / bismuth ferrite heterojunction.
[0032] In some embodiments, the alkaline solution is selected from one of potassium hydroxide and sodium hydroxide.
[0033] In some embodiments, after the first mixed solution and the alkaline solution are mixed, stirring is further performed, and the stirring time is 1 to 6 hours.
[0034] By stirring, the first mixed solution and the alkaline solution in the preparation system can be fully mixed to generate bismuth hydroxide and iron hydroxide.
[0035] Step 3: Use microwave to assist the second mixed solution in hydrothermal reaction, the temperature of the hydrothermal reaction is 140-180° C., the time is 30-50 min, to obtain an intermediate product.
[0036] The microwave-assisted hydrothermal reaction of the second mixed solution refers to using microwaves as a heating tool in the hydrothermal reaction. The microwave-assisted hydrothermal reaction can achieve rapid temperature rise to the temperature required for material crystallization and growth, which is conducive to shortening the reaction time.
[0037] On the one hand, the present application also improves the iron oxide / bismuth ferrite heterojunction based on in-situ growth by controlling the hydrothermal reaction temperature and reaction time. Specifically, the present application found that when the reaction temperature is low, the crystal growth power is insufficient, and a complete and uniform BiFeO3 crystal cannot be generated in a short time, or the bismuth ferrite crystal tends to be Bi 25 FeO 40 The probability of independent growth of iron oxide is small. Properly increasing the reaction temperature is beneficial to providing good conditions for uniform and rapid growth of BiFeO3 crystals and Fe2O3 crystals, thereby facilitating the acquisition of iron oxide / bismuth ferrite heterojunction based on in-situ growth.
[0038] The present application also found that in the initial stage of the reaction, when the reaction time is short, it is not conducive to the formation of BiFeO3 crystal structure, or it is easy to form a small amount of Bi 25 FeO 40 Properly extending the reaction time is conducive to the in-situ growth of iron in the form of Fe2O3 crystals, but when the reaction time is too long, the Fe2O3 crystals decrease, which is speculated to be due to the conversion of Fe2O3 into BiFeO3-type bismuth ferrite. Therefore, controlling the reaction time within a suitable range is conducive to the successful construction of an iron oxide / bismuth ferrite heterojunction based on in-situ growth.
[0039] Step 4: Wash and dry the intermediate product to obtain the iron oxide / bismuth ferrite heterojunction material.
[0040] In some embodiments, the drying temperature is 50-80° C. and the drying time is 6-24 hours.
[0041] Different from the prior art that prepares heterojunctions by physical mixing, the present application uses microwave-assisted hydrothermal reaction to achieve rapid heating to reach the temperature required for material crystallization and growth, which is conducive to shortening the reaction time. Moreover, by controlling the ratio of bismuth to iron, the concentration of the alkaline solution, the hydrothermal reaction temperature and the reaction time, while synthesizing bismuth ferrite, iron oxide grows in situ on the surface of bismuth ferrite to achieve the construction of an iron oxide / bismuth ferrite heterojunction, so that the atoms between the interfaces form good contact, which is conducive to optimizing the material interface and improving the time-space separation efficiency of carriers, thereby obtaining a photocatalyst material with higher catalytic efficiency.
[0042] Another embodiment of the present application further provides an iron oxide / bismuth ferrite heterojunction material prepared by the preparation method.
[0043] In the iron oxide / bismuth ferrite heterojunction material of the present application, iron oxide forms a composite structure with bismuth ferrite in an in-situ growth manner, has a higher quality material interface, and further improves the time and space separation efficiency of carriers. Therefore, the iron oxide / bismuth ferrite heterojunction material of the present application has excellent photocatalytic activity. Compared with the same type of materials, its oxygen production performance is 2 to 3 times that of non-heterostructures.
[0044] The scheme of the present application will be explained below in conjunction with the embodiments. Those skilled in the art will understand that the following examples are only used to explain the present application and cannot be construed as limiting the present application. Unless otherwise stated, the reagents, software and instruments not specifically stated in the following embodiments are all conventional commercial products or open source.
[0045] Embodiment 1:
[0046] In this example, an iron oxide / bismuth ferrite heterojunction material is prepared, and the preparation method includes:
[0047] Step 1: Add 0.0125 mol of bismuth nitrate and 0.0125 mol of ferric nitrate (the molar ratio of bismuth nitrate to ferric nitrate is 1:1) and 0.05 mol of nitric acid to 50 mL of deionized water, stir at 25 ° C for 1 hour, and then slowly add dropwise to 4 M potassium hydroxide using a dropper while continuing to stir. After stirring at 25 ° C for 1 hour, ultrasonic vibration is performed for 10 minutes, and the ultrasonic temperature does not exceed 50 ° C. Then, stir at 25 ° C for another 1 hour to obtain a mixed solution having a reddish-brown precipitate.
[0048] Step 2: Transfer the mixed solution obtained in step 1 to a polytetrafluoroethylene reactor, and subject it to microwave hydrothermal reaction at 180° C. for 30 min to obtain an intermediate product.
[0049] Step 3: centrifuge and wash the intermediate product obtained in step 2 with deionized water and ethanol to a pH of 5-7, and then dry at 50-80° C. for 6-24 hours to obtain the final product, i.e., iron oxide / bismuth ferrite heterojunction material.
[0050] The present application has carried out transmission electron microscopy analysis and X-ray diffraction analysis on the iron oxide / bismuth ferrite heterojunction material obtained in Example 1. Figure 1 and Figure 2 The lattice spacing of the (101) crystal plane of bismuth ferrite is consistent with the crystal plane spacing corresponding to the peak at 22.4° in the X-ray diffraction spectrum, proving that this substance is indeed bismuth ferrite. Its edge is closely connected with another form of substance, indicating that this substance grows in situ on the surface of bismuth ferrite. Figure 2 The results analysis show that the product obtained after microwave-assisted hydrothermal reaction is composed of bismuth ferrite and iron oxide.
[0051] The present application further uses an energy dispersive X-ray spectrometer to analyze the iron oxide / bismuth ferrite heterojunction material obtained in Example 1, see Figure 3 The results showed that the substance in direct contact with bismuth ferrite was mainly composed of two elements, iron and oxygen, and did not contain bismuth. It can be preliminarily determined that this heterogeneous component is iron oxide.
[0052] The above results indicate that iron oxide grows in situ on the surface of bismuth ferrite during the microwave-assisted hydrothermal process to form a heterostructure.
[0053] Embodiment 2:
[0054] The difference from Example 1 is that the molar ratio of the bismuth nitrate to the ferric nitrate is adjusted to 1.5:1.
[0055] Embodiment 3:
[0056] The difference from Example 1 is that the molar ratio of the bismuth nitrate to the ferric nitrate is adjusted to 1:2.
[0057] Comparative Example 1:
[0058] The difference from Example 1 is that the molar ratio of the bismuth nitrate to the ferric nitrate is adjusted to 1:4.
[0059] Comparative Example 2:
[0060] The difference from Example 1 is that the molar ratio of the bismuth nitrate to the ferric nitrate is adjusted to 2:1.
[0061] Comparative Example 3:
[0062] The difference from Example 1 is that the molar ratio of the bismuth nitrate to the ferric nitrate is adjusted to 4:1.
[0063] The present application conducted X-ray diffraction analysis on the final products obtained in Examples 1-3 and Comparative Examples 1-3. Figure 4 , Fe2O3 was detected in the final products of Examples 1-3, but not in Comparative Examples 1-3. After analysis, the molar ratio of bismuth to iron in Comparative Example 1 was low (1:4), and the insufficient bismuth content made it difficult to form BiFeO3 with a complete crystal structure, reducing the separation efficiency of carriers. The molar ratio of bismuth to iron in Comparative Example 2 was high (2:1). Since the solubility of Fe(OH)3 generated in the preparation process in water is lower than that of Bi(OH)3, during the reaction, the bismuth content in the solution is higher, and it occupies a dominant position in the molecular collision and competition process, and is more inclined to form a crystal form of Bi 25 FeO 40In the process of bismuth ferrite, Fe2O3 participates in the crystal formation and cannot achieve independent in-situ growth on the surface of bismuth ferrite crystal. In comparative example 3, the molar ratio of bismuth to iron is too high, the bismuth element content is too high, and it precipitates in the form of crystals. This result shows that when the molar ratio of bismuth to iron is controlled at 1:2 to 1.5:1, it is easier to generate Fe2O3 crystals, which is conducive to the construction of iron oxide / bismuth ferrite heterojunction based on in-situ growth.
[0064] Furthermore, the present application has carried out a photocatalytic activity test on the final products obtained in Examples 1-3 and Comparative Examples 1-2. The oxygen production system consists of a fully automatic gas generation glass system, a xenon lamp light source, a vacuum pump and a condensing device. Through the automatic control program of the equipment, the main valve of the equipment is turned every 30 minutes when the equipment is working to connect the pipeline connected to the chromatographic carrier gas. Under the suction force of the vacuum pump, the gas generated by the reactor is transported to the high-performance gas chromatography by the carrier gas for analysis, and the component analysis results are displayed by the electrical signal of the chromatographic workstation. In the process of photocatalytic water oxidation performance testing, 10 mg of the sample was dispersed in 30 mL of Na2S2O8 (0.1M) solution and then ultrasonicated for 10 minutes to form a uniform dispersion system of the photocatalyst. Turn on the hydrogen evolution equipment, carrier gas source, chromatograph and computer workstation in sequence, pour the sample dispersion solution into the quartz window reaction vessel of the photocatalytic instrument, maintain a stirring rate of 1000r / min, close the reaction vessel, control the reaction temperature at 5°C through the circulating condensed water system, shine the xenon lamp light source equipped with UVCUT420 filter on the reaction vessel for visible light irradiation, turn on the vacuum pump for about 20 minutes of vacuum extraction, and then start sampling to test the photocatalytic oxygen production performance. After the main valve of the equipment is turned 7 times, the sample oxygen production performance results of 3h are obtained. The results are fitted with the standard curve to obtain the final oxygen production performance data, please refer to Figure 5 The final product of Example 1-3 has a significantly better oxygen production effect than that of Comparative Example 1-2, indicating that controlling the molar ratio of the bismuth source to the iron source in the range of 1:2 to 1.5:1 during the preparation process is beneficial to obtaining a composite structure formed by Fe2O3 and BiFeO3 in an in-situ growth manner. By in-situ constructing an atomic-sharing heterojunction, good contact is formed between the atoms at the interface, which is more conducive to promoting charge transfer and efficient spatiotemporal separation of carriers, further improving the photocatalytic performance of the composite material, and can be applied to photocatalytic hydrolysis to produce oxygen, degradation of organic pollutants, and organic synthesis as a photocatalyst.
[0065] Embodiment 4:
[0066] The difference from Example 1 is that the concentration of potassium hydroxide is adjusted to 8M.
[0067] Embodiment 5:
[0068] The difference from Example 1 is that the concentration of potassium hydroxide is adjusted to 2M.
[0069] Comparative Example 4:
[0070] The difference from Example 1 is that the concentration of potassium hydroxide is adjusted to 1M.
[0071] Comparative Example 5:
[0072] The difference from Example 1 is that the concentration of potassium hydroxide is adjusted to 10M.
[0073] The present application conducted X-ray diffraction analysis on the final products obtained in Example 1, Examples 4-5 and Comparative Examples 4-5 using different concentrations of alkaline solutions. Figure 6 , Fe2O3 was detected in Example 1 and Example 4-5, but not in Comparative Example 4-5. After analysis, the alkaline solution acts as a mineralizer in the microwave hydrothermal process, which can improve the crystallinity of bismuth ferrite under short-term high temperature and high pressure conditions. As the concentration of the mineralizer increases, the probability of bismuth in the preparation example system combining with iron to form R3C bismuth ferrite increases. Therefore, when the concentration of the alkaline solution is too low (Comparative Example 4), the bismuth ferrite crystal structure is not completely formed, and when the concentration of the alkaline solution is too high (Comparative Example 5), the iron element tends to participate in the construction of other crystal forms of bismuth ferrite, and it is difficult for the Fe2O3 crystal to grow independently in situ on the BiFeO3 surface. Thus, it is shown that the concentration of the alkaline solution affects the formation of the heterojunction between bismuth ferrite and iron oxide. Controlling the alkaline solution within the range of 2M to 8M is conducive to the formation of bismuth ferrite with a crystal form of BiFeO3, and is also conducive to the iron element appearing in the form of Fe2O3 crystals, which is conducive to the construction of an iron oxide / bismuth ferrite heterojunction based on in-situ growth.
[0074] Embodiment 6:
[0075] The difference from Example 1 is that the temperature of the microwave hydrothermal reaction is adjusted to 140°C.
[0076] Embodiment 7:
[0077] The difference from Example 1 is that the temperature of the microwave hydrothermal reaction is adjusted to 160°C.
[0078] Comparative Example 6:
[0079] The difference from Example 1 is that the temperature of the microwave hydrothermal reaction is adjusted to 120°C.
[0080] Comparative Example 7:
[0081] The difference from Example 1 is that the temperature of the microwave hydrothermal reaction is adjusted to 200°C.
[0082] The present application has carried out X-ray diffraction analysis on the final products obtained in Example 1, Examples 6-7 and Comparative Examples 6-7 at different hydrothermal reaction temperatures. Please refer to Figure 7 Fe2O3 was detected in Examples 1 and 6-7, but not in Comparative Examples 6-7. After analysis, it was found that when the temperature was low, such as in Comparative Example 6, the bismuth ferrite crystals tended to be Bi 25 FeO 40 The probability of independent growth of iron oxide is small, and the crystal growth power is insufficient, so complete and uniform bismuth ferrite crystals cannot be generated in a short time. However, as shown in Comparative Example 7, the temperature should not be too high. This result shows that a suitable high temperature and high pressure environment provides good conditions for the uniform and rapid growth of BiFeO3, and is conducive to the appearance of iron elements in the form of Fe2O3 crystals, which is conducive to the construction of an iron oxide / bismuth ferrite heterojunction based on in-situ growth.
[0083] Embodiment 8:
[0084] The difference from Example 1 is that the time of the microwave hydrothermal reaction is adjusted to 40 min.
[0085] Embodiment 9:
[0086] The difference from Example 1 is that the time of the microwave hydrothermal reaction is adjusted to 50 min.
[0087] Comparative Example 8:
[0088] The difference from Example 1 is that the time of the microwave hydrothermal reaction is adjusted to 10 min.
[0089] Comparative Example 9:
[0090] The difference from Example 1 is that the time of the microwave hydrothermal reaction is adjusted to 20 min.
[0091] Comparative Example 10:
[0092] The difference from Example 1 is that the time of the microwave hydrothermal reaction is adjusted to 60 min.
[0093] The present application has carried out X-ray diffraction analysis on the final products obtained in Example 1, Examples 8-9 and Comparative Examples 8-10 with different hydrothermal reaction times. Please refer to Figure 8 Fe2O3 was detected in Examples 1 and 8-9, but not in Comparative Examples 8-10. After analysis, it was found that the reaction time was insufficient, or it could be understood that in the initial stage of the reaction, the growth time was too short, which was not conducive to the formation of BiFeO3 crystal structure. As the reaction time progressed, a small amount of Bi 25 FeO 40Type bismuth ferrite; appropriately extend the reaction time, such as in Examples 1, 8-9, there are relatively obvious iron oxide crystals; but as the reaction time continues to extend, Fe2O3 gradually disappears. It is speculated that when the reaction time is long enough and the temperature is suitable, the iron element combines with the bismuth element to form BiFeO3 type bismuth ferrite, and Fe2O3 is completely converted to form pure phase BiFeO3 type bismuth ferrite. This result shows that under suitable reaction conditions, BiFeO3 type bismuth ferrite and independent Fe2O3 crystals are formed in a certain reaction stage, and controlling the reaction time within the range of 30 to 50 minutes is more conducive to the construction of iron oxide / bismuth ferrite heterojunction based on in-situ growth.
[0094] The above implementation modes are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application has been described in detail with reference to the above preferred implementation modes, a person skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.
Claims
1. A method for preparing an iron oxide / bismuth ferrite heterojunction material, characterized in that: The preparation method comprises: Mixing a bismuth source compound, an iron source compound and an acid solution, wherein the molar ratio of bismuth in the bismuth source compound to iron in the iron source compound is 1:2 to 1.5:1, to obtain a first mixed solution; Providing an alkaline solution with a concentration of 2M to 8M, mixing the first mixed solution with the alkaline solution, so that the bismuth in the bismuth source compound and the iron in the iron source compound form bismuth hydroxide and iron hydroxide respectively, to obtain a second mixed solution; Using microwave to assist the second mixed solution to perform a hydrothermal reaction, wherein the temperature of the hydrothermal reaction is 140 to 180° C. and the time is 30 to 50 min to obtain an intermediate product; The intermediate product is washed and dried to obtain the iron oxide / bismuth ferrite heterojunction material.
2. The preparation method according to claim 1, characterized in that The bismuth source compound is selected from one or more of bismuth nitrate and its hydrate, bismuth sulfate and its hydrate, and bismuth acetate and its hydrate.
3. The preparation method according to claim 1, characterized in that: The iron source compound is selected from one or more of ferric nitrate and its hydrate, ferric sulfate and its hydrate, and ferric acetate and its hydrate.
4. The preparation method according to claim 1, characterized in that: The acid solution includes nitric acid.
5. The preparation method according to claim 1, characterized in that: The temperature of the alkaline solution is 25-30°C.
6. The preparation method according to claim 1, characterized in that: The alkaline solution is selected from one of potassium hydroxide and sodium hydroxide.
7. The preparation method according to claim 1, characterized in that: After the first mixed solution and the alkaline solution are mixed, stirring is further performed, and the stirring time is 1 to 6 hours.
8. The preparation method according to claim 1, characterized in that: The drying temperature is 50-80° C. and the drying time is 6-24 hours.
9. An iron oxide / bismuth ferrite heterojunction material, characterized in that: The iron oxide / bismuth ferrite heterojunction material is prepared by the preparation method according to any one of claims 1 to 8.