Cu-doped Bi2WO6 photocatalyst as well as preparation method and application thereof
The hydrothermal preparation of Cu-doped Bi2WO6 photocatalyst solves the problem of low efficiency of pure Bi2WO6 photocatalyst, significantly improves its catalytic activity and CO2 reduction performance under visible light, and is suitable for industrial applications.
Patent Information
- Application Number
- CN202410720770.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The photocatalytic efficiency of pure Bi2WO6 photocatalyst is low, and the development efficiency of sunlight is low and the massive recombination of light-generated charges makes it difficult to meet the industrial CO2 reduction performance requirements.
Cu-doped Bi2WO6 photocatalyst is prepared by hydrothermal method. The Cu doping amount is 1-2% of Bi2WO6, forming Cu-doped Bi2WO6 with improved energy band structure, which improves the visible light response and catalytic activity of the photocatalyst.
The visible light response and catalytic activity of the photocatalyst are significantly improved, and the photocatalytic reduction ability is enhanced, especially the performance in reducing carbon dioxide to carbon monoxide. The preparation method is simple and low-cost, and is suitable for large-scale production.
Smart Images

Figure CN118719081A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalytic materials, and specifically relates to a Cu-doped Bi2WO6 photocatalyst and a preparation method and application thereof. Background Art
[0002] Due to the rapid advancement of industrialization, energy crisis and environmental pollution have become major challenges facing the world. Solar energy, as a clean energy with great development prospects, has attracted much attention. Converting solar energy into chemical energy through photocatalysts can solve both energy and environmental pollution problems. Converting CO2 into hydrocarbon fuels and value-added chemical products such as CO and CH4 can effectively reduce environmental pollution and alleviate the energy crisis. Using only sunlight and water, CO2 reduction can be produced on the surface of semiconductors. This green and pollution-free method has attracted more and more attention. In recent years, a large number of semiconductor material studies have been conducted on CO2 reduction. However, based on the inherent properties of these materials, the performance of CO2 reduction is far from meeting the needs of industrialization.
[0003] Bi2WO6 has attracted extensive attention and application due to its significant advantages of simple synthesis, environmental friendliness, good stability and suitable band structure. However, the photocatalytic efficiency of pure Bi2WO6 photocatalysts is usually limited, mainly due to its significantly lower efficiency in sunlight development and a large amount of recombination of photogenerated charges. Therefore, people have designed a variety of modification techniques to improve the photocatalytic efficiency of Bi2WO6 photocatalytic carbon dioxide reduction, but there are no reports on Cu-doped Bi2WO6 as a photocatalyst for carbon dioxide reduction. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the present invention provides a Cu-doped Bi2WO6 photocatalyst and a preparation method and application thereof.
[0005] The technical solution adopted by the present invention is:
[0006] A Cu-doped Bi2WO6 photocatalyst, wherein the doping amount of Cu is 1-2% of Bi2WO6 in terms of molar percentage.
[0007] The above-mentioned method for preparing a Cu-doped Bi2WO6 photocatalyst includes the following steps: adding Bi(NO3)3·5H2O and Na2WO4·2H2O to a mixed solution of water and ethylene glycol, and stirring to form a uniform precursor solution; adding CuSO4·5H2O to the precursor solution, stirring evenly, transferring to a high-pressure reactor, performing a hydrothermal reaction, cooling to room temperature after the reaction is completed, centrifuging and washing, and drying to obtain a Cu-doped Bi2WO6 photocatalyst.
[0008] Preferably, in the above-mentioned preparation method, the molar ratio is Bi(NO3)3·5H2O:Na2WO4·2H2O=2:1.
[0009] Preferably, in the above-mentioned preparation method, the mixed solution of water and ethylene glycol has a volume ratio of water:ethylene glycol=1:1.
[0010] Preferably, in the above-mentioned preparation method, the hydrothermal reaction conditions are: reaction at 120° C. for 24 hours.
[0011] Preferably, in the above preparation method, the drying temperature is 60°C.
[0012] The above-mentioned Cu-doped Bi2WO6 photocatalyst is used to catalyze the reduction of carbon dioxide to carbon monoxide under visible light irradiation.
[0013] Furthermore, the above application method is as follows: put the Cu-doped Bi2WO6 photocatalyst and deionized water into an alumina crucible, evaporate after mixing, and form a uniform film; put it into a reactor, evacuate it, fill it with carbon dioxide gas, and irradiate it under visible light conditions.
[0014] Furthermore, for the above application, Cu-doped Bi2WO6:deionized water = 20 mg:0.5 mL.
[0015] The beneficial effects of the present invention are:
[0016] 1. The present invention uses a hydrothermal method to prepare a Cu-doped Bi2WO6 photocatalyst. After Cu doping modification, impurity energy levels are generated in the original energy band structure, which reduces the electron transition barrier, can effectively reduce the recombination of photogenerated electrons and holes, and improve the separation efficiency of carriers, thereby significantly improving the visible light response of the catalyst and enhancing the photocatalytic activity.
[0017] 2. The Cu-doped Bi2WO6 photocatalyst prepared by the present invention has a larger specific surface area and a more effective photogenerated electron and hole separation ability, as well as a stronger photocatalytic reduction ability, participates in the catalytic reaction, and is an effective way to improve the visible light catalytic activity.
[0018] 3. The Cu-doped Bi2WO6 photocatalyst prepared by the present invention has good photocatalytic carbon dioxide reduction performance, and the method is simple, convenient, low-cost, mild conditions, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 X-ray diffraction patterns of Bi2WO6, Bi2WO6-1%Cu and Bi2WO6-2%Cu photocatalysts prepared in Example 1.
[0020] Figure 2This is the photocurrent-time curve of the Bi2WO6, Bi2WO6-1%Cu and Bi2WO6-2%Cu photocatalysts prepared in Example 1.
[0021] Figure 3 This is a comparison chart of the activity of Bi2WO6, Bi2WO6-1%Cu and Bi2WO6-2%Cu photocatalysts prepared in Example 1 for reducing carbon dioxide to carbon monoxide. DETAILED DESCRIPTION
[0022] Example 1 Cu-doped Bi2WO6 photocatalyst (I) Preparation of Bi2WO6
[0023] 1.5mmol Bi(NO3)3·5H2O and 0.75mmol Na2WO4·2H2O were placed in a mixed solution of 30mL water and 30mL ethylene glycol, stirred to form a uniform precursor solution, and then placed in a hydrothermal autoclave for hydrothermal reaction at 120°C for 24h, naturally cooled to room temperature, washed three times with distilled water, and dried at 60°C to obtain Bi2WO6.
[0024] (II) Preparation of Bi2WO6 photocatalyst with 1% Cu doping
[0025] 1.5mmol Bi(NO3)3·5H2O and 0.75mmol Na2WO4·2H2O were placed in a mixed solution of 30mL water and 30mL ethylene glycol, and stirred to form a uniform precursor solution. Then, 0.0074mmol CuSO4·5H2O was added, and after being fully stirred, it was transferred to a high-pressure reactor and subjected to hydrothermal reaction at 120°C for 24h. After the reaction was completed, it was naturally cooled to room temperature, washed three times by centrifugation with distilled water, and dried at 60°C to obtain a Bi2WO6 photocatalyst with a Cu doping amount of 1%, which was marked as Bi2WO6-1%Cu.
[0026] (III) Preparation of Bi2WO6 photocatalyst with 2% Cu doping
[0027] 1.5mmol Bi(NO3)3·5H2O and 0.75mmol Na2WO4·2H2O were placed in a mixed solution of 30mL water and 30mL ethylene glycol, and stirred to form a uniform precursor solution. Then, 0.0149mmol CuSO4·5H2O was added, and after being fully stirred, it was transferred to a high-pressure reactor and subjected to hydrothermal reaction at 120°C for 24h. After the reaction was completed, it was naturally cooled to room temperature, washed three times by centrifugation with distilled water, and dried at 60°C to obtain a Bi2WO6 photocatalyst with a Cu doping amount of 2%, which was marked as Bi2WO6-2%Cu.
[0028] (IV) Testing
[0029] Figure 1X-ray diffraction patterns of Bi2WO6, Bi2WO6-1%Cu and Bi2WO6-2%Cu photocatalysts prepared in Example 1. Figure 1 In the 5 significant characteristic diffraction peaks at 2θ=28.3°, 32.7°, 47.1°, 55.8° and 58.5°, they correspond to the (131), (002), (202), (331) and (262) crystal planes of Bi2WO6, respectively (standard card PDF#79-2381). Figure 1 No characteristic peaks of other impurities were observed, indicating that the original structure of Bi2WO6 was still retained after Cu doping Bi2WO6 on the surface.
[0030] Example 2 Application of Cu-doped Bi2WO6 photocatalyst in catalytic reduction of carbon dioxide to carbon monoxide under light
[0031] The method is as follows: 20 mg of Bi2WO6, Bi2WO6-1%Cu and Bi2WO6-2%Cu photocatalysts prepared in Example 1 and 0.5 mL of deionized water are respectively placed in an alumina crucible, mixed and evaporated to form a uniform film. At room temperature and pressure, the crucible is placed in a container, 0.5 mL of deionized water is added to the bottom of the container, the container is sealed, the container is evacuated and filled with carbon dioxide gas, and under visible light irradiation conditions, 1000 μL of gas in the container is taken with a micro syringe every 60 minutes, and the sample gas components are detected by gas chromatography separation technology to determine the carbon monoxide concentration.
[0032] Figure 2 The photocurrent-time curves of Bi2WO6, Bi2WO6-1%Cu and Bi2WO6-2%Cu photocatalysts prepared in Example 1. The results show that the photocurrent intensity of Bi2WO6-2%Cu is about 5.14μA·cm -2 , is pure Bi2WO6 (0.75μA·cm -2 ) times of that of the semiconductor. This indicates that doping with Cu improves the separation efficiency of photogenerated carriers in the semiconductor, thereby improving the photoelectrochemical performance of the semiconductor.
[0033] Figure 3 This is a comparison chart of the activity of Bi2WO6, Bi2WO6-1%Cu and Bi2WO6-2%Cu photocatalysts prepared in Example 1 in reducing carbon dioxide to carbon monoxide. Figure 3It can be seen that after 4 hours of light reaction, the CO production of Bi2WO6 is 1122.39μmol / g, the CO production of Bi2WO6-1%Cu is 1307.79μmol / g, and the CO production of Bi2WO6-2%Cu is 2633.09μmol / g. The catalytic carbon monoxide production performance of Bi2WO6 photocatalyst doped with Cu is greatly improved compared with pure Bi2WO6. This shows that after Cu doping Bi2WO6, the photogenerated electron transfer ability is stronger, and the electron holes have stronger redox ability.
Claims
1. A Cu-doped Bi2WO6 photocatalyst, characterized in that: In terms of molar percentage, the doping amount of Cu is 1-2% of Bi2WO6.
2. The method for preparing a Cu-doped Bi2WO6 photocatalyst according to claim 1, characterized in that: The method comprises the following steps: adding Bi(NO3)3·5H2O and Na2WO4·2H2O to a mixed solution of water and ethylene glycol, and stirring to form a uniform precursor solution; adding CuSO4·5H2O to the precursor solution, stirring evenly, and transferring to a high-pressure reactor to perform a hydrothermal reaction, cooling to room temperature after the reaction is completed, centrifugally washing, and drying to obtain a Cu-doped Bi2WO6 photocatalyst.
3. The preparation method according to claim 2, characterized in that: In molar ratio, Bi(NO3)3·5H2O:Na2WO4·2H2O=2:
1.
4. The preparation method according to claim 2, characterized in that: The mixed solution of water and ethylene glycol has a volume ratio of water:ethylene glycol=1:
1.
5. The preparation method according to claim 2, characterized in that: The hydrothermal reaction conditions are: 120° C. for 24 hours.
6. The preparation method according to claim 2, characterized in that: The drying temperature is 60°C.
7. Use of the Cu-doped Bi2WO6 photocatalyst according to claim 1 in catalyzing the reduction of carbon dioxide to carbon monoxide under visible light irradiation.
8. The use according to claim 7, characterized in that: The method is as follows: Cu-doped Bi2WO6 photocatalyst and deionized water are placed in an alumina crucible, mixed and evaporated to form a uniform film; the film is placed in a reactor, evacuated and filled with carbon dioxide gas, and irradiated under visible light conditions.
9. The use according to claim 8, characterized in that: Cu-doped Bi2WO6: deionized water = 20 mg: 0.5 mL.
Citation Information
Patent Citations
Preparation of copper-doped bismuth tungstate photocatalyst
CN113769754A
Preparation method for controlling morphology of different Bi2WO6 photocatalysts at low temperature
CN114522678A
Carbon quantum dot / bismuth tungstate heterojunction and preparation method and application thereof
CN116688974A
Cited By
Cu-doped MnMoO4 photocatalyst as well as preparation method and application thereof
CN119897123A