W modified Ni / gamma-Al2O3 catalyst for methanation of carbon dioxide as well as preparation and application of W modified Ni / gamma-Al2O3 catalyst

By preparing W-modified Ni/γ-Al2O3 catalyst, the problem of insufficient low-temperature activity of nickel-based catalysts was solved, the catalytic activity of carbon dioxide methanation reaction was significantly improved, and efficient CO2 conversion rate was achieved.

CN118719082APending Publication Date: 2024-10-01SHANGHAI INST OF TECH

Patent Information

Application Number
CN202410764835.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Nickel-based catalysts have insufficient low-temperature activity in carbon dioxide methanation reactions, which limits their application effects.

Method used

The W-modified Ni/γ-Al2O3 catalyst is prepared by adding a mixed aqueous solution of Ni salt and W salt dropwise into the γ-Al2O3 powder, followed by impregnation, drying and roasting. An appropriate amount of W element is added to improve the activity and activity of the catalyst. Selectivity.

Benefits of technology

It effectively improves the CO2 methanation catalytic activity of the catalyst and increases the CO2 conversion rate. Especially under the appropriate W addition amount, the CO2 conversion rate of the catalyst is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719082A_ABST
    Figure CN118719082A_ABST
Patent Text Reader

Abstract

The invention relates to a W modified Ni / gamma-Al2O3 catalyst for methanation of carbon dioxide and preparation and application thereof, the catalyst takes gamma-Al2O3 as a carrier, takes metal Ni as an active component and takes W as an auxiliary component, the content of the metal Ni is 8-12% of the mass of the carrier, and the mass of the W is 0.03-0.3% of the mass of the carrier. By adding W, the catalytic activity of CO2 methanation is improved, and the catalyst is particularly suitable for catalyzing CO2 hydrogenation to synthesize methane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon dioxide to methane synthesis, and relates to a W-modified Ni / γ-Al2O3 catalyst for carbon dioxide methanation, and a preparation method and application thereof. Background Art

[0002] Excessive carbon dioxide emissions can lead to the greenhouse effect. At the same time, CO2 is also a carbon resource with abundant reserves, cheap and easy to obtain. It is crucial to achieve resource utilization of CO2 while reducing emissions. CO2 hydrogenation to methane is an important way to utilize CO2 resources, and CO2 methanation reaction has become a research hotspot.

[0003] Catalyst is the core of CO2 methanation process, and the performance of catalyst directly determines the effect of CO2 methanation. Precious metal catalysts are expensive, so their application is limited. Among non-metallic catalysts, nickel (Ni)-based catalysts have become widely used catalysts in CO2 methanation reactions due to their excellent catalytic performance, abundant resources, and relatively low prices. However, the low-temperature activity of nickel-based catalysts still needs to be improved. Adding suitable additives to nickel-based catalysts can improve the properties of the catalyst, improve the catalyst activity, selectivity and stability, etc. The present invention is also proposed based on this. Summary of the invention

[0004] The purpose of the present invention is to provide a W-modified Ni / γ-Al2O3 catalyst for carbon dioxide methanation and its preparation and application, so as to improve the catalytic activity of CO2 methanation.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] In one aspect, the present invention provides a W-modified Ni / γ-Al2O3 catalyst for carbon dioxide methanation, which uses γ-Al2O3 as a carrier, metal Ni as an active component, and W as an auxiliary component, wherein the content of metal Ni is 8-12% of the carrier mass, and the mass of the W element is 0.03-0.3% of the carrier mass.

[0007] On the other hand, the present invention provides a method for preparing a W-modified Ni / γ-Al2O3 catalyst for carbon dioxide methanation, wherein a mixed aqueous solution of Ni salt and W salt is first added dropwise to γ-Al2O3 powder and stirred evenly, and then impregnated, dried, and calcined to obtain the catalyst.

[0008] Furthermore, the impregnation process adopts an equal volume impregnation method.

[0009] Furthermore, the Ni salt is Ni(NO3)2·6H2O.

[0010] Further, the W salt is (NH4) 10 (H2W 12 O 42 )·4H2O.

[0011] Furthermore, the stirring process is carried out at room temperature.

[0012] Furthermore, the immersion time is 2-4 hours, preferably 3 hours.

[0013] Further, the drying temperature is 100-120°C and dried overnight, preferably 110°C.

[0014] Furthermore, the calcination process is: heating from room temperature to 450-550°C at a heating rate of 4-6°C / min, and calcining for 3-5h, preferably, heating from room temperature to 500°C at a heating rate of 5°C / min, and calcining for 4h.

[0015] On the other hand, the present invention also provides an application of a W-modified Ni / γ-Al2O3 catalyst for carbon dioxide methanation in catalytic carbon dioxide hydrogenation to methane.

[0016] Specifically, the application process is as follows: the catalyst is mixed with quartz sand in a mass ratio of 1:3, stirred evenly, and loaded into a quartz reaction tube, the catalyst is first reduced with H2 / N2 (molar ratio of 10%), and then a reaction gas containing CO2 and H2 is introduced at 250-450°C to react to obtain methane.

[0017] Compared with the prior art, the present invention can effectively improve the catalytic activity of Ni / γ-Al2O3 catalyst for CO2 methanation by adding W. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is the carbon dioxide conversion rate of the xW-Ni / γ-Al2O3 catalyst prepared in Examples 1 to 5 and Comparative Example 1, wherein (A) x=0.03; (B) x=0.05; (C) x=0.1; (D) x=0.3; (E) x=0.5; (F) x=0. DETAILED DESCRIPTION

[0019] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0020] The gases used in the following examples and comparative examples were from Shanghai Weichuang Standard Gas Co., Ltd., and other reagents were purchased from Sinopharm Shanghai Reagent Company, and all reagents were of analytical grade.

[0021] The models, specifications, manufacturers and other information of the equipment and analytical instruments used in the following embodiments and comparative examples are shown in Table 1.

[0022] Table 1 Models, specifications and manufacturers of instruments used

[0023]

[0024] Embodiment 1:

[0025] A W-modified Ni / γ-Al2O3 catalyst uses γ-Al2O3 as a carrier, metal Ni as an active component, and W as an auxiliary agent, wherein the content of Ni accounts for 10% of the carrier mass, and the content of W accounts for 0.03% of the carrier mass.

[0026] The preparation method of the above catalyst comprises the following specific steps:

[0027] (1) Weigh 1.0g of Ni(NO3)2·6H2O and 0.009g of (NH4) 10 (H2W 12 O 24 )·4H2O is placed in a crucible, and 4.0 g of deionized water is added to dissolve it to form a mixed aqueous solution of nickel salt and tungsten salt;

[0028] (2) Add the mixed aqueous solution of nickel salt and tungsten salt obtained in step (1) dropwise to 2 g of γ-Al2O3 powder, stir evenly at room temperature, soak for 3 h, move into a drying oven, and dry at 110°C overnight;

[0029] (3) The mixture obtained in step (2) was transferred to a muffle furnace, and the temperature was raised from room temperature to 500° C. at a heating rate of 5° C. / min and calcined for 4 h to obtain W-modified Ni / γ-Al 2 O 3 catalyst A.

[0030] Example 2

[0031] A W-modified Ni / γ-Al2O3 catalyst uses γ-Al2O3 as a carrier, metal Ni as an active component, and W as an auxiliary agent, wherein the content of Ni accounts for 10% of the carrier mass, and the content of W accounts for 0.05% of the carrier mass.

[0032] In the above-mentioned method for preparing the catalyst, only the (NH4) weighed in step (1) is adjusted. 10 (H2W 12 O 24 )·4H2O mass, so that the mass of W accounts for 0.05% of the mass of the carrier. Other aspects are the same as in Example 1, to obtain W-modified Ni / γ-Al2O3 catalyst B.

[0033] Example 3

[0034] A W-modified Ni / γ-Al2O3 catalyst uses γ-Al2O3 as a carrier, metal Ni as an active component, and W as an auxiliary agent, wherein the content of Ni accounts for 10% of the carrier mass, and the content of W accounts for 0.1% of the carrier mass.

[0035] In the above-mentioned method for preparing the catalyst, only the (NH4) weighed in step (1) is adjusted. 10 (H2W 12 O 24 )·4H2O mass, so that the mass of W accounts for 0.1% of the mass of the carrier. Other aspects are the same as in Example 1, to obtain a W-modified Ni / γ-Al2O3 catalyst C.

[0036] Example 4

[0037] A W-modified Ni / γ-Al2O3 catalyst uses γ-Al2O3 as a carrier, metal Ni as an active component, and W as an auxiliary agent, wherein the content of Ni accounts for 10% of the carrier mass, and the content of W accounts for 0.3% of the carrier mass.

[0038] In the above-mentioned method for preparing the catalyst, only the (NH4) weighed in step (1) is adjusted. 10 (H2W 12 O 24 )·4H2O mass, so that the mass of W accounts for 0.3% of the mass of the carrier. Other aspects are the same as in Example 1, to obtain W-modified Ni / γ-Al2O3 catalyst D.

[0039] Example 5

[0040] A W-modified Ni / γ-Al2O3 catalyst uses γ-Al2O3 as a carrier, metal Ni as an active component, and W as an auxiliary agent, wherein the content of Ni accounts for 10% of the carrier mass, and the content of W accounts for 0.5% of the carrier mass.

[0041] In the above-mentioned method for preparing the catalyst, only the (NH4) weighed in step (1) is adjusted. 10 (H2W 12 O 24 )·4H2O mass, so that the mass of W accounts for 0.5% of the mass of the carrier. Other aspects are the same as in Example 1, and a W-modified Ni / γ-Al2O3 catalyst E is obtained.

[0042] Comparative Example 1

[0043] γ-Al2O3 is used as a carrier, and metal Ni is an active component, wherein the content of Ni accounts for 10% of the carrier mass.

[0044] The preparation method of the above catalyst specifically comprises the following steps:

[0045] (1) Weigh 1.0 g of Ni(NO3)2·6H2O into a crucible, add 4 g of deionized water to dissolve it, and form a Ni(NO3)2 aqueous solution;

[0046] (2) Add the Ni(NO3)2 aqueous solution obtained in step (1) dropwise to 2 g of γ-Al2O3 powder, stir evenly at room temperature, soak for 3 h, move into a drying oven, and dry at 110°C overnight;

[0047] (3) The mixture obtained in step (2) was transferred to a muffle furnace, and the temperature was raised from room temperature to 500° C. at a heating rate of 5° C. / min and calcined for 4 h to obtain Ni / γ-Al 2 O 3 catalyst F.

[0048] Application Example 1

[0049] An example of the process of the present invention for the hydrogenation of carbon dioxide to methane is described below.

[0050] 0.15 g of each catalyst A, B, C, D, E and F obtained in Examples 1 to 5 and Comparative Example 1 were mixed with 0.45 g of quartz sand and filled into quartz reaction tubes respectively. In a 10% H2 / N2 mixed gas with a flow rate of 30 ml / min, the temperature was raised from room temperature to 500°C at a rate of 5°C / min and the mixture was reduced at a constant temperature for 3 h. After the temperature was lowered to 250°C, the gas was switched to the reaction gas (CO2:H2=1:4) with a reaction gas flow rate of 60 ml / min and a space velocity of 24000 ml·g -1 ·h -1 The reaction temperature range is 250~450℃. The catalyst activity test results are as follows Figure 1 shown.

[0051] The catalysts A, B and C obtained in Examples 1 to 5 have a better effect of catalyzing CO2 to methane than the catalyst F in Comparative Example 1. When the amount of W added is 0.05% (catalyst B), the CO2 conversion rate of the catalyst reaches 82.7% at 350°C (the CO2 conversion rate of catalyst F is 66.7%). As the amount of W added continues to increase, the CO2 conversion rate on the catalyst decreases. In summary, the catalyst used for CO2 hydrogenation to methane prepared by adding a suitable additive in the present invention has a high catalytic activity for the CO2 hydrogenation to methane reaction and has a good development prospect.

[0052] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A W-modified Ni / γ-Al for CO2 methanation 2 O 3 catalyst, It is characterized in that Its γ-Al 2 O 3 As a carrier, metal Ni is used as an active component and W is used as an auxiliary component, wherein the content of metal Ni is 8-12% of the carrier mass, and the mass of W element is 0.03-0.3% of the carrier mass.

2. A W-modified Ni / γ-Al for carbon dioxide methanation according to claim 1 2 O 3 A method for preparing a catalyst, It is characterized in that First, add the mixed aqueous solution of Ni salt and W salt to the γ-Al 2 O 3 The powder is stirred evenly, and then impregnated, dried and calcined to obtain the catalyst.

3. A W-modified Ni / γ-Al for carbon dioxide methanation according to claim 2 2 O 3 A method for preparing a catalyst, It is characterized in that The impregnation process adopts the equal volume impregnation method.

4. A W-modified Ni / γ-Al for carbon dioxide methanation according to claim 2 2 O 3 A method for preparing a catalyst, It is characterized in that The Ni salt is Ni(NO 3 ) 2 6H 2 O.

5. A W-modified Ni / γ-Al for carbon dioxide methanation according to claim 2 2 O 3 A method for preparing a catalyst, It is characterized in that The W salt is (NH 4 ) 10 (H 2 W 12 O 42 )·4H 2 O.

6. A W-modified Ni / γ-Al for carbon dioxide methanation according to claim 2 2 O 3 A method for preparing a catalyst, It is characterized in that The stirring process was carried out at room temperature.

7. A W-modified Ni / γ-Al for carbon dioxide methanation according to claim 2 2 O 3 A method for preparing a catalyst, It is characterized in that The immersion time is 2-4 hours.

8. A W-modified Ni / γ-Al for carbon dioxide methanation according to claim 2 2 O 3 A method for preparing a catalyst, It is characterized in that The drying temperature was 100-120°C and dried overnight.

9. A W-modified Ni / γ-Al for carbon dioxide methanation according to claim 2 2 O 3 A method for preparing a catalyst, It is characterized in that The calcination process is as follows: heating from room temperature to 450-550°C at a heating rate of 4-6°C / min, and calcining for 3-5h.

10. The W-modified Ni / γ-Al for carbon dioxide methanation according to claim 1 2 O 3 Application of catalyst in catalytic hydrogenation of carbon dioxide to methane.

Citation Information

Patent Citations

  • Anti-carbon synthesis gas methanation catalyst, preparation method and application thereof

    CN104353463A

  • CO selective methanation method

    CN111974405A

  • Carbon dioxide (CO2) methanation catalyst as well as preparation method and application thereof

    CN113368862A

  • Catalyst for reforming mathand and carbon dioxide to synthesize gas

    CN1344671A

  • Co2 methanation catalyst and method for producing the same, and method for producing methane

    JP2022094211A

Cited By

  • Preparation method of nano-catalyst based on bimetal organic framework material as well as product and application of nano-catalyst

    CN119524928A