Regeneration method of silver catalyst for preparing ethylene oxide through ethylene epoxidation and preparation method of ethylene oxide
By impregnating and roasting the silver catalyst, the problems of rising reaction temperature and declining selectivity in the regeneration of the ethylene oxidation catalyst are solved, the recovery of catalyst performance and the improvement of economic benefits are achieved, and the generation of waste liquid and waste gas is avoided.
Patent Information
- Application Number
- CN202310342201.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, the regeneration research of ethylene oxidation catalyst has not been effectively solved, which leads to an increase in reaction temperature and a decrease in selectivity during use of the catalyst. Frequent replacement of the catalyst is required, and the recycling process consumes high energy and produces waste liquid and waste gas.
By immersing the silver catalyst in the silver-containing impregnating solution, draining and roasting, the activity and selectivity of the catalyst are restored, avoiding the recycling of the old catalyst, saving time and costs.
It effectively restores part or most of the performance of the catalyst, extends the service life of the catalyst, reduces economic costs, and avoids the generation of waste liquid and waste gas.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst regeneration, and more specifically to a method for regenerating a silver catalyst used in preparing ethylene oxide by epoxidation of ethylene and a method for preparing ethylene oxide. Background Art
[0002] Under the action of silver catalyst, ethylene oxidation mainly produces ethylene oxide, and byproducts such as carbon dioxide and water are also produced. Among them, activity, selectivity and stability are the main performance indicators of silver catalysts. Activity refers to the reaction temperature required for the ethylene oxide production process to reach a certain reaction load. The lower the reaction temperature, the higher the activity of the catalyst; selectivity refers to the ratio of the number of moles of ethylene converted into ethylene oxide to the total number of moles of ethylene in the reaction; stability is expressed as the rate of decrease of activity and selectivity. The smaller the rate of decrease, the better the stability of the catalyst. Using high-activity, high-selectivity and good-stability silver catalysts in the process of ethylene oxidation to produce ethylene oxide can greatly improve economic benefits. Therefore, the manufacture of high-activity, high-selectivity and good-stability silver catalysts is the main direction of silver catalyst research.
[0003] As the ethylene epoxidation catalyst continues to operate, the growth of silver catalyst particles causes the reaction temperature of the catalyst to rise and the selectivity to decrease, proving that the catalyst has reached the end of its life and needs to be replaced. Therefore, research on catalyst regeneration is of great significance, but no research on the regeneration of ethylene epoxidation catalyst has been conducted so far.
[0004] Silver catalyst recovery usually uses nitric acid leaching to extract silver, and then recovers it. The carrier is also crushed for other uses. This method of recovering catalysts is not only economically energy-intensive, but also produces waste liquid, waste gas and waste solids during the recovery process. Summary of the invention
[0005] The object of the present invention is to provide a method for regenerating a silver catalyst used in preparing ethylene oxide by epoxidation of ethylene, wherein the catalyst is immersed in a silver-containing impregnation solution, and then the catalyst is drained and calcined to regenerate the catalyst.
[0006] In order to achieve the above-mentioned object, the present invention provides a method for regenerating a silver catalyst for preparing ethylene oxide by epoxidation of ethylene, the regeneration method comprising: impregnating the silver catalyst for preparing ethylene oxide by epoxidation of ethylene in a silver-containing impregnation solution; then draining and roasting to obtain a regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
[0007] Another aspect of the present invention provides a method for preparing ethylene oxide, which comprises: regenerating a silver catalyst for preparing ethylene oxide by epoxidation of ethylene according to the above-mentioned regeneration method to obtain a regenerated catalyst; and then allowing ethylene and oxygen to undergo epoxidation reaction in the presence of the regenerated catalyst to obtain ethylene oxide.
[0008] The technical solution of the present invention has the following beneficial effects:
[0009] (1) The regeneration method of the present invention can regenerate the catalyst by immersing the catalyst in a silver-containing impregnation solution, draining and calcining the catalyst, and the regenerated catalyst can continue to be used for ethylene epoxidation reaction.
[0010] (2) The regeneration method proposed by the present invention can reduce the size of silver nanoparticles on the surface of the silver catalyst by adjusting the impregnation liquid during regeneration, and the regenerated catalyst recovers part or most of the catalytic performance and can continue to be used for ethylene epoxidation reaction. It avoids the recycling of old catalyst, saves time and cost, and has good economic benefits.
[0011] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0012] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein.
[0013] One aspect of the present invention provides a method for regenerating a silver catalyst for preparing ethylene oxide by epoxidation of ethylene. The regeneration method comprises: impregnating the silver catalyst for preparing ethylene oxide by epoxidation of ethylene in a silver-containing impregnation solution; then draining and roasting to obtain a regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
[0014] According to the present invention, preferably, the silver-containing impregnation solution comprises a silver compound, an organic amine, a rhenium auxiliary, water, an optional alkali metal auxiliary and an optional co-auxiliary;
[0015] Wherein, the mass ratio of the organic amine to water is 1:(1-5);
[0016] Based on the total weight of the silver-containing impregnation solution, the silver content is 0.5%-10%, preferably 0.5%-5%; the rhenium content is 5-500ppm, preferably 10-150ppm; the alkali metal content is 0-400ppm, preferably 5-100ppm; the co-auxiliary content in terms of metal elements is 0-200ppm, preferably 5-100ppm.
[0017] According to the present invention, the organic amine can be any organic amine compound suitable for preparing a silver catalyst for ethylene oxide, as long as the organic amine compound can form a silver amine complex with a silver compound. Preferably, the organic amine is selected from at least one of pyridine, butylamine, ethylenediamine, 1,3-propylenediamine, ethanolamine and triethylamine.
[0018] According to the present invention, preferably, the silver compound is selected from silver oxide and / or silver salt, and the silver salt is preferably selected from silver nitrate and / or silver carbonate, and further preferably selected from silver carbonate;
[0019] The rhenium-containing auxiliary agent is selected from at least one of rhenium element, rhenium oxide, perrhenic acid and perrhenate, preferably selected from perrhenic acid and / or perrhenate; the perrhenate is preferably selected from cesium perrhenate and / or ammonium perrhenate.
[0020] According to the present invention, preferably, the alkali metal auxiliary agent is at least one of nitrates, sulfates and hydroxides of alkali metals; the alkali metal is at least one of lithium, sodium, potassium, rubidium and cesium; the co-auxiliary agent is at least one of chromium element, molybdenum element, tungsten element, boron element, chromium metal compounds, molybdenum metal compounds, tungsten metal compounds and boron compounds.
[0021] According to the present invention, preferably, the calcination temperature is 200-450°C;
[0022] The calcination is performed in an oxygen-containing atmosphere, preferably in air.
[0023] In the present invention, preferably, the calcination time is 0.5-30h.
[0024] In the present invention, the impregnated silver catalyst is activated and thermally decomposed at 200-450° C. by calcination.
[0025] In the present invention, the oxygen-containing atmosphere is an air atmosphere and / or a nitrogen-oxygen mixed gas atmosphere with an oxygen mass content of no more than 21%.
[0026] According to the present invention, preferably, the silver content of the regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene is increased by 0.5-10%, preferably by 0.5-5%, based on the total weight of the regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
[0027] According to the present invention, preferably, before impregnation, the particle size of the silver nanoparticles in the silver catalyst for preparing ethylene oxide by epoxidation of ethylene is 500-1500 nm.
[0028] Judging from the catalytic performance of the catalyst, in the present invention, the silver catalyst for preparing ethylene oxide by epoxidation of ethylene before impregnation refers to a catalyst whose original reaction temperature rises to above 250° C. and whose selectivity is less than 87%.
[0029] According to the present invention, preferably, the silver catalyst for preparing ethylene oxide by epoxidation of ethylene comprises silver nanoparticles, a carrier and an optional auxiliary agent;
[0030] The additive is preferably at least one of a rhenium additive, a cesium additive, a chromium additive and a molybdenum additive.
[0031] In the present invention, the content of the supported silver nanoparticles is 10 to 40 wt % based on the total weight of the silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
[0032] In the present invention, "catalyst regeneration" refers to the process of restoring the efficiency of a catalyst whose catalytic efficiency has declined. The regeneration process does not involve the disintegration of the overall structure of the catalyst, but only uses appropriate methods to eliminate the factors that cause the catalytic efficiency to decline.
[0033] The above silver catalyst for preparing ethylene oxide by epoxidation of ethylene can be prepared by conventional methods in the art, for example but not limited to, loading silver nanoparticles onto a carrier by an impregnation method to obtain a catalyst.
[0034] Another aspect of the present invention provides a method for preparing ethylene oxide, which comprises: regenerating a silver catalyst for preparing ethylene oxide by epoxidation of ethylene according to the above-mentioned regeneration method to obtain a regenerated catalyst; and then allowing ethylene and oxygen to undergo epoxidation reaction in the presence of the regenerated catalyst to obtain ethylene oxide.
[0035] The present invention is further described below by examples:
[0036] In the following preparation examples and embodiments, the evaluation method of the silver catalyst performance is as follows:
[0037] The various ethylene epoxidation catalysts involved in the following preparation examples, embodiments and comparative examples were tested for their activity and selectivity using a laboratory microreactor (hereinafter referred to as "microreactor") evaluation device. The reactor used in the microreactor evaluation device is a stainless steel tube with an inner diameter of 4 mm, and the reaction tube is placed in a heating jacket. The catalyst loading volume is 1 mL, and there is an inert filler at the bottom so that the catalyst bed is located in the constant temperature zone of the heating jacket.
[0038] In the following preparation examples and embodiments, the conditions for measuring the catalyst activity and selectivity are shown in Table 1:
[0039] Table 1 Determination conditions of catalyst activity and selectivity
[0040]
[0041] When the above reaction conditions are stably reached, the gas composition at the reactor inlet and outlet is continuously measured. The selectivity S is calculated according to the following formula after volume shrinkage correction is performed on the measured results:
[0042]
[0043] Among them, ΔEO is the difference in ethylene oxide concentration between the reactor outlet gas and the inlet gas, ΔCO2 is the difference in carbon dioxide concentration between the reactor outlet gas and the inlet gas, and the average of more than 10 groups of test data is taken as the test result of the day.
[0044] In the following Table 2, the test method for the size of silver particles on the surface of the silver catalyst before regeneration or after regeneration is as follows: Under a scanning electron microscope, the size of the silver particles is visually tested and counted, and then a normal distribution curve of the silver particle size is drawn based on the statistical data, and the median value of the particle size on the normal distribution curve is used as the value of the silver particle size on the silver catalyst surface.
[0045] The silver content was determined by chemical titration.
[0046] Vector Preparation Example
[0047] 190g of α-trihydrate Al2O3 with a mesh size of 50-500, 210g of pseudo-monohydrate Al2O3 with a mesh size of more than 200, 5g of aluminum fluoride, 0.9g of SiO2, and 3.0g of barium oxide were put into a mixer and mixed evenly. Then, the mixture was transferred to a kneader, and 150 ml of dilute nitric acid (nitric acid: water = 1:5, weight ratio) was added and kneaded into a paste that can be extruded. The mixture was extruded into a five-hole columnar object with an outer diameter of 8.0mm, a length of 6.0mm, and an inner diameter of 1.0mm. The mixture was dried at 80-120℃ for more than 2 hours to reduce the free water content to less than 10%. Then, the green body was placed in an electric furnace and kept at 250℃ for 12 hours. Then, the green body was taken out and cooled to room temperature. After about 18 hours, the temperature was raised from room temperature to 1460℃ and kept constant for 4 hours to obtain a white α-Al2O3 carrier sample.
[0048] Catalyst Preparation Example 1
[0049] Take 7.0g of silver nitrate and dissolve it in 10mL of deionized water. Add 1g of triethylamine and 5g of deionized water to a stirred glass flask. Slowly add the prepared silver nitrate solution to the triethylamine aqueous solution while stirring, keep the temperature below 45°C, so that all the silver nitrate is dissolved, add 0.1g of ammonium perrhenate, and then add deionized water to make the total mass of the solution reach 20g to prepare an impregnation mixture. The amount of silver nitrate added is such that the impregnation mixture contains 24.5wt% silver.
[0050] Take 4g of the α-alumina particles prepared in the carrier preparation example, put the carrier α-alumina particles into 10g of the impregnation mixture prepared above, put it into a vacuum container, evacuate to a vacuum degree of more than 10mmHg, immerse the carrier and keep it for 30 minutes, and leach out the excess solution. The leached carrier is heated in an air flow at 210°C for 30 minutes and cooled to prepare a silver catalyst for ethylene oxide.
[0051] Catalyst Preparation Example 2
[0052] The catalyst in Catalyst Preparation Example 1 was used to prepare ethylene oxide under the conditions shown in Table 1 of the above-mentioned method for evaluating the performance of the silver catalyst, and the process was carried out under the conditions shown in Table 1 for 1045 days.
[0053] Catalyst Preparation Example 3
[0054] The catalyst in Catalyst Preparation Example 1 was used to prepare ethylene oxide under the conditions shown in Table 1 of the above-mentioned method for evaluating the performance of silver catalysts, and the process was carried out under the conditions shown in Table 1 for 1600 days.
[0055] Catalyst Regeneration Example 1
[0056] Take 0.35g of silver nitrate and dissolve it in 10mL of deionized water. Add 1g of triethylamine and 5g of deionized water in a stirred glass flask. Slowly add the prepared silver nitrate solution to the mixture under stirring, keep the temperature below 45°C, so that all the silver nitrate is dissolved, and then add deionized water to make the total mass of the solution reach 20g to prepare the impregnation mixture. The amount of silver nitrate added is such that the impregnation mixture contains 1.5wt% silver.
[0057] Take 4g of the catalyst in Catalyst Preparation Example 2, put the catalyst into 10g of the impregnation mixture prepared above, put it into a vacuum container, evacuate to a vacuum degree of more than 10mmHg, immerse the catalyst and keep it for 30 minutes, and leach out the excess solution. The leached catalyst is heated in an air flow at 210°C for 30 minutes, and cooled to obtain a regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
[0058] The catalyst was loaded into a reactor with a catalyst loading amount of 0.1 g, and then evaluated according to the above-mentioned silver catalyst performance evaluation method.
[0059] Catalyst Regeneration Example 2
[0060] Take 0.35g of silver nitrate and dissolve it in 10mL of deionized water. Add 1g of triethylamine and 5g of deionized water to a stirred glass flask. Slowly add the prepared silver nitrate solution to the mixture while stirring, keep the temperature below 45°C, so that all the silver nitrate is dissolved, add 0.04g of cesium perrhenate and 0.02g of potassium nitrate, and then add deionized water to make the total mass of the solution reach 20g to prepare an impregnation mixture. The amount of silver nitrate added is such that the impregnation mixture contains 1.5wt% silver.
[0061] Take 4g of the catalyst in Catalyst Preparation Example 2, put the catalyst into 10g of the impregnation mixture prepared above, put it into a vacuum container, evacuate to a vacuum degree of more than 10mmHg, immerse the catalyst and keep it for 30 minutes, and leach out the excess solution. The leached catalyst is heated in an air flow at 210°C for 30 minutes, and cooled to obtain a regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
[0062] The catalyst was loaded into a reactor with a catalyst loading amount of 0.1 g, and then evaluated according to the above-mentioned silver catalyst performance evaluation method.
[0063] Catalyst Regeneration Example 3
[0064] Take 1.75g of silver nitrate and dissolve it in 10mL of deionized water. Add 1g of triethylamine and 5g of deionized water to a stirred glass flask. Slowly add the prepared silver nitrate solution to the mixture while stirring, keep the temperature below 45°C, so that all the silver nitrate is dissolved, add 0.04g of cesium perrhenate and 0.02g of potassium nitrate, and then add deionized water to make the total mass of the solution reach 20g to prepare an impregnation mixture. The amount of silver nitrate added is such that the impregnation mixture contains 5.0wt% silver.
[0065] Take 4g of the catalyst in Catalyst Preparation Example 2, put the catalyst into 10g of the impregnation mixture prepared above, put it into a vacuum container, evacuate to a vacuum degree of more than 10mmHg, immerse the catalyst and keep it for 30 minutes, and leach out the excess solution. The leached catalyst is heated in an air flow at 210°C for 30 minutes, and cooled to obtain a regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
[0066] The catalyst was loaded into a reactor with a catalyst loading amount of 0.1 g, and then evaluated according to the above-mentioned silver catalyst performance evaluation method.
[0067] Catalyst Regeneration Example 4
[0068] Take 3.15g of silver nitrate and dissolve it in 10mL of deionized water. Add 1g of triethylamine and 5g of deionized water to a stirred glass flask. Slowly add the prepared silver nitrate solution to the mixture while stirring, keep the temperature below 45°C, and dissolve all the silver nitrate. Add 0.04g of cesium perrhenate and 0.02g of potassium nitrate, and then add deionized water to make the total mass of the solution reach 20g to prepare an impregnation mixture. The amount of silver nitrate added is such that the impregnation mixture contains 9wt% silver.
[0069] Take 4g of the catalyst in Catalyst Preparation Example 2, put the catalyst into 10g of the impregnation mixture prepared above, put it into a vacuum container, evacuate to a vacuum degree of more than 10mmHg, immerse the catalyst and keep it for 30 minutes, and leach out the excess solution. The leached catalyst is heated in an air flow at 210°C for 30 minutes, and cooled to obtain a regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
[0070] The catalyst was loaded into a reactor with a catalyst loading amount of 0.1 g, and then evaluated according to the above-mentioned silver catalyst performance evaluation method.
[0071] Catalyst Regeneration Example 5
[0072] Take 1.75g of silver nitrate and dissolve it in 10mL of deionized water. Add 1g of triethylamine and 5g of deionized water to a stirred glass flask. Slowly add the prepared silver nitrate solution to the mixture while stirring, keep the temperature below 45°C, so that all the silver nitrate is dissolved, add 0.04g of cesium perrhenate and 0.02g of potassium nitrate, and then add deionized water to make the total mass of the solution reach 20g to prepare an impregnation mixture. The amount of silver nitrate added is such that the impregnation mixture contains 5wt% silver.
[0073] Take 4g of the catalyst in Catalyst Preparation Example 3, put the catalyst into 10g of the impregnation mixture prepared above, put it into a vacuum container, evacuate to a vacuum degree of more than 10mmHg, immerse the catalyst and keep it for 30 minutes, and leach out the excess solution. The leached catalyst is heated in an air flow at 210°C for 30 minutes, and cooled to obtain a regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
[0074] The catalyst was loaded into a reactor with a catalyst loading amount of 0.1 g, and then evaluated according to the above-mentioned silver catalyst performance evaluation method.
[0075] The activity and selectivity of the catalyst samples were measured using a microreactor evaluation device under the process conditions shown in Table 1. The test results are listed in Table 2
[0076] Table 2 Test results of catalysts used in catalyst preparation examples 2-3 and catalyst regeneration examples 1-5 for producing ethylene oxide by ethylene oxidation
[0077]
[0078] *Note: Selective EO production reaches 400T / M 3 The average value of the catalyst.
[0079] By comparing the data in Table 2, increasing the silver content in the impregnation solution and increasing the addition of additives have an important influence on the catalyst regeneration effect; the impregnation silver concentration should not be too large, which will increase the size of silver particles, affect the catalytic performance, and increase the production cost; the results show that regeneration by the method proposed in the present invention can effectively restore the catalytic performance of the catalyst.
[0080] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for regenerating a silver catalyst for preparing ethylene oxide by epoxidation of ethylene, characterized in that: The regeneration method comprises: impregnating the silver catalyst for preparing ethylene oxide by epoxidation of ethylene in a silver-containing impregnation solution; then draining and roasting to obtain the regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
2. The regeneration method according to claim 1, wherein: The silver-containing impregnation solution comprises a silver compound, an organic amine, a rhenium auxiliary agent, water, an optional alkali metal auxiliary agent and an optional co-auxiliary agent; Wherein, the mass ratio of the organic amine to water is 1:(1-5); Based on the total weight of the silver-containing impregnation solution, the silver content is 0.5%-10%, preferably 0.5%-5%; the rhenium content is 5-500ppm, preferably 10-150ppm; the alkali metal content is 0-400ppm, preferably 5-100ppm; the co-auxiliary content in terms of metal elements is 0-200ppm, preferably 5-100ppm.
3. The regeneration method according to claim 2, wherein: The organic amine is at least one selected from pyridine, butylamine, ethylenediamine, 1,3-propylenediamine, ethanolamine and triethylamine.
4. The regeneration method according to claim 2, wherein: The silver compound is selected from silver oxide and / or silver salt, and the silver salt is preferably selected from silver nitrate and / or silver carbonate, and further preferably selected from silver carbonate; The rhenium-containing auxiliary agent is selected from at least one of rhenium element, rhenium oxide, perrhenic acid and perrhenate, preferably selected from perrhenic acid and / or perrhenate; the perrhenate is preferably selected from cesium perrhenate and / or ammonium perrhenate.
5. The regeneration method according to claim 2, wherein: The alkali metal auxiliary agent is at least one of nitrates, sulfates and hydroxides of alkali metals; the alkali metal is at least one of lithium, sodium, potassium, rubidium and cesium; The co-additive is at least one of chromium, molybdenum, tungsten, boron, chromium metal compounds, molybdenum metal compounds, tungsten metal compounds and boron compounds.
6. The regeneration method according to claim 1, wherein: The calcination temperature is 200-450°C; The calcination is performed in an oxygen-containing atmosphere, preferably in air.
7. The regeneration method according to claim 1, wherein: The silver content of the regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene is increased by 0.5-10%, preferably by 0.5-5%, based on the total weight of the regenerated silver catalyst for preparing ethylene oxide by epoxidation of ethylene.
8. The regeneration method according to claim 1, wherein: Before impregnation, the particle size of the silver nanoparticles in the silver catalyst for preparing ethylene oxide by epoxidation of ethylene is 500-1500 nm.
9. The regeneration method according to claim 1, wherein: The silver catalyst for preparing ethylene oxide by epoxidation of ethylene comprises silver nanoparticles, a carrier and an optional auxiliary agent; The additive is preferably at least one of a rhenium additive, a cesium additive, a chromium additive and a molybdenum additive.
10. A method for preparing ethylene oxide, characterized in that: The preparation method comprises: regenerating a silver catalyst used for preparing ethylene oxide by epoxidation of ethylene according to the regeneration method described in any one of claims 1 to 9 to obtain a regenerated catalyst; and then causing ethylene and oxygen to undergo epoxidation reaction in the presence of the regenerated catalyst to obtain ethylene oxide.
Citation Information
Patent Citations
Preparation method of silver catalyst for producing ethylene oxide, silver catalyst prepared thereby and application thereof
CN102527384A
Ag catalyst for producing epoxyethane, its preparation method and uses
CN1803279A
Reactivation of an exhausted catalyst body - by impregnating it with a soln. of a caesium or rubidium cpd.
DE2611856B1
Cited By
Preparation method and application of double-interface electrocatalyst for preparing ethylene oxide
CN120738681A