Regeneration method of waste silver catalyst for ethylene oxide preparation through ethylene oxidation, regenerated silver catalyst and application
Through solvent treatment and impregnation activation technology, the activity and selectivity of the waste silver catalyst are improved, the problem of decreased catalyst activity is solved, the service life is extended, the production cost is reduced, and a green and environmentally friendly process is realized.
Patent Information
- Application Number
- CN202310343165.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology has limited effect in improving the activity and selectivity of spent silver catalysts, and the improvement in catalyst performance is not significant enough, especially the problem of decreased catalyst activity after long-term use.
Using solvent treatment, ultrasonic, centrifugation, drying and impregnation activation with silver-containing impregnation solution, the waste silver catalyst is treated through inert organic solvents and/or water, combined with organic amines, alkali metal additives, alkaline earth metal additives and rhenium additives. The impregnation liquid is impregnated and activated, which significantly improves the activity and selectivity of the catalyst.
The activity and selectivity of the waste silver catalyst are significantly improved, the service life of the catalyst is extended, the production cost is reduced, and a green and environmentally friendly process is realized.
Smart Images

Figure BDA0004158947200000071 
Figure BDA0004158947200000072 
Figure BDA0004158947200000151
Abstract
Description
Technical Field
[0001] The invention belongs to the field of regeneration of waste silver catalysts, and in particular relates to a regeneration method for a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, a regenerated silver catalyst and an application thereof. Background Art
[0002] Direct oxidation of ethylene under the action of silver catalyst mainly produces ethylene oxide (EO), while side reactions occur to produce carbon dioxide and water, etc. Among them, activity, selectivity and stability are the main performance indicators of silver catalysts. The so-called activity refers to the reaction temperature required when the ethylene oxide production process reaches a certain reaction load. The lower the reaction temperature, the higher the activity of the catalyst. The so-called selectivity refers to the ratio of the number of moles of ethylene converted into ethylene oxide in the reaction to the total number of moles of ethylene in the reaction. The so-called stability is expressed as the rate of decrease of activity and selectivity. The smaller the rate of decrease, the better the stability of the catalyst. For industrial catalysts, stability and life are crucial. The stability of industrial catalysts includes three aspects: thermal stability, chemical stability and mechanical stability. In theory, the catalyst can change the rate of chemical reaction, and it does not enter the product itself. It keeps the physical and chemical properties unchanged before and after the reaction, and can work continuously in a cycle. However, in actual reactions, the catalyst cannot be used indefinitely. Although it is only a short-term participant, under the action of long-term heat and chemistry, some physical and chemical changes will occur, resulting in a decrease in catalyst activity and ultimately catalyst deactivation. Temperature has many effects on solid catalysts. It can cause the active components to volatilize and drain, the supported metal to sinter or the micro-crystals to grow, etc., resulting in a decrease in catalyst activity. On the active surface of some catalysts, due to the interference of side reactions such as hydrogenolysis, polymerization, cyclization and hydrogen transfer, surface contamination, blockage or coking can also cause a decrease in catalyst activity. A decrease in catalyst activity will cause an increase in reaction temperature, a decrease in selectivity, and a shortened catalyst life.
[0003] Silver catalysts for direct oxidation of ethylene to produce ethylene oxide are divided into three categories: high-activity silver catalysts, medium-high selectivity silver catalysts and high-selectivity silver catalysts. The initial selectivity of the high-activity silver catalyst is 80-81 mol%, the final selectivity is 76-78 mol%, and the space-time yield can reach 280 gEO / h*liter of catalyst; the initial selectivity of the medium-high selectivity silver catalyst is 81-85 mol%, the highest selectivity is 85-86 mol%, the final selectivity is 80-82 mol%, and the space-time yield can reach 200-280 gEO / h*liter of catalyst; the initial selectivity of the high-selectivity silver catalyst is 82-85 mol%, the highest selectivity is 87-92 mol%, the final selectivity is 82-84 mol%, and the space-time yield can reach 160-220 gEO / h*liter of catalyst.
[0004] In recent years, some process technologies for improving the activity of silver catalysts have emerged. Patent US6372925B1 found that for aged high-selectivity catalysts, the activity and selectivity of the catalyst can be improved by increasing the concentration of ethylene. Patent US7348444B2 and CN100482652C proposed that before the catalyst reaches the highly aged stage, the reaction temperature is increased to above 255°C, and the ethylene content of the feed is increased to above 25 mol% relative to the total feed, thus improving the performance of the catalyst, especially the activity, selectivity and stability.
[0005] Methods for improving the activity and / or selectivity of spent silver catalysts are mostly based on post-treatment or regeneration of spent catalysts. Post-treatment, for example, comprises impregnating the spent catalyst with a solution comprising water, a water-miscible solvent and a cesium and / or rubidium compound. The catalyst impregnated in this way is dried and then the catalyst dried in this way is used again in the oxidation reaction. Such methods have been described, for example, in DE2519599, DE2611856, DE2636680, DE2649359, EP0101008 and DE2938245. In the regeneration methods described in US4529714 or US4391735, the silver-containing catalyst is treated in a very similar manner; but here the regeneration solution also contains hydrazine and / or aliphatic or aromatic acids as additives. US4125480 washes the used catalyst with 1-10 times its volume of water or a mixture of water and an organic solvent before the additional promoter is deposited on the catalyst, but treatment with water or an aqueous solution has an adverse effect on the catalyst performance. US4186106 washes the catalyst with an inert organic liquid and then applies cesium, rubidium or a mixture thereof to the catalyst, the use of such a non-aqueous solvent can provide adequate cleaning of the catalyst and eliminate the problem of exposure of the catalyst and / or reactor to an aqueous environment. US6624116 describes an in-situ regeneration method, the catalyst is used in an autothermal oxidation process for converting paraffins to olefins, the regeneration is achieved by introducing a vaporizable compound of a Group 8b metal and / or by introducing a vaporizable co-catalyst into the reactor together with the reaction mixture.
[0006] The above methods not only adjust the composition of the reaction gas, but also use a solution containing water, a water-miscible solvent and a cesium and / or rubidium compound to impregnate the spent catalyst to improve the performance of the low-activity or spent silver catalyst. However, these methods have limited improvement on the activity and selectivity of the low-activity or spent silver catalyst. Therefore, there is still a need to develop a method for regenerating spent silver catalysts in the art. Summary of the invention
[0007] In view of the above-mentioned state of the prior art, the inventors of the present invention have conducted extensive and in-depth research in the field of silver catalysts and the field of ethylene oxidation to ethylene oxide. As a result, it is found that the waste silver catalyst can be regenerated by successively subjecting the waste silver catalyst to solvent treatment, ultrasound, centrifugation, drying and activation by impregnation with a silver-containing impregnation solution, which is not only green and environmentally friendly, but also can significantly reduce the production cost of the silver catalyst.
[0008] In order to achieve the purpose of the present invention, the first aspect of the present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0009] (1) adding a waste silver catalyst for preparing ethylene oxide by oxidation of ethylene to a solvent to obtain a solid-liquid mixture; the solvent is an inert organic solvent and / or water;
[0010] (2) subjecting the solid-liquid mixture obtained in step (1) to ultrasonic treatment to obtain an ultrasonically treated solid-liquid mixture;
[0011] (3) centrifuging and drying the solid-liquid mixture after ultrasonic treatment obtained in step (2) to obtain a substrate;
[0012] (4) obtaining an impregnation solution comprising a silver-containing compound, an organic amine, water, an alkali metal additive, an alkaline earth metal additive, an optional rhenium additive and a co-additive thereof;
[0013] (5) The substrate obtained in step (3) is impregnated with the impregnation solution in step (4), and then activated by leaching to obtain a regenerated silver catalyst.
[0014] The second aspect of the present invention provides a regenerated silver catalyst obtained by the regeneration method.
[0015] The third aspect of the present invention provides an application of the regenerated silver catalyst in the production of ethylene oxide by oxidation of ethylene.
[0016] The regenerated silver catalyst of the present invention can improve the activity, selectivity and service life of the waste silver catalyst in the process of producing ethylene oxide by ethylene oxidation; it also makes the production process green and environmentally friendly; and it can significantly reduce the production cost of the silver catalyst.
[0017] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0018] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0019] One of the objects of the present invention is to provide a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0020] (1) adding a waste silver catalyst for preparing ethylene oxide by oxidation of ethylene to a solvent to obtain a solid-liquid mixture; the solvent is an inert organic solvent and / or water;
[0021] (2) subjecting the solid-liquid mixture obtained in step (1) to ultrasonic treatment to obtain an ultrasonically treated solid-liquid mixture;
[0022] (3) centrifuging the solid-liquid mixture after ultrasonic treatment obtained in step (2), and drying it to obtain a substrate;
[0023] (4) obtaining an impregnation solution comprising a silver-containing compound, an organic amine, water, an alkali metal additive, an alkaline earth metal additive, an optional rhenium additive and a co-additive thereof;
[0024] (5) The substrate obtained in step (3) is impregnated with the impregnation solution in step (4), and then activated by leaching to obtain a regenerated silver catalyst.
[0025] According to the present invention, preferably, in step (1), the mass ratio of the solvent to the waste silver catalyst for preparing ethylene oxide by oxidation of ethylene is 1 to 20:1, preferably 1.5 to 15:1, and more preferably 2 to 10:1.
[0026] According to the present invention, preferably, in step (1), the waste silver catalyst for ethylene oxidation to ethylene oxide is a silver catalyst for ethylene oxidation to ethylene oxide at the end of the reaction, preferably a medium-to-high selectivity silver catalyst or a high-activity silver catalyst at the end of the reaction, and more preferably a medium-to-high selectivity silver catalyst or a high-activity silver catalyst with a reaction temperature higher than 250°C.
[0027] In the present invention, the regenerable waste silver catalyst for producing ethylene oxide by ethylene oxidation includes but is not limited to the following models: YS-8520, YS-8520H, YS-8520G, and YS-7.
[0028] According to the present invention, preferably, in step (1), the inert organic solvent is selected from at least one of C1-C6 fatty alcohols, C6-C8 fatty hydrocarbons and C6-C8 alicyclic hydrocarbons, preferably selected from at least one of methanol, ethanol, isopropanol, n-hexane and cyclohexane; and the water is deionized water.
[0029] According to the present invention, preferably, in step (2), the ultrasonic treatment is carried out in an ultrasonic device; preferably, the ultrasonic device is an ultrasonic cleaning machine, the power of the ultrasonic treatment is 35 to 18000 W, preferably 100 to 500 W, the temperature is 10 to 80° C., and the time is 0.1 to 99 min, preferably 5 to 20 min.
[0030] According to the present invention, preferably, in step (3), the centrifugal treatment is carried out in a centrifuge, and preferably, the rotation speed of the centrifugal treatment is 100 to 16500 rpm, and the time is 1 to 100 min.
[0031] According to the present invention, preferably, in step (3), the drying temperature is 30 to 150° C. and the drying time is 0.1 to 10 h.
[0032] According to the present invention, preferably, in step (4), the silver-containing compound is selected from at least one of silver nitrate, silver acetate and silver oxalate.
[0033] According to the present invention, preferably, in step (4), the organic amine is selected from at least one of ethylamine, ethylenediamine, n-propylamine, 1,3-propylenediamine, n-butylamine, 1,4-butylenediamine, ethanolamine and propanolamine.
[0034] According to the present invention, preferably, in step (4), the alkali metal auxiliary agent is at least one selected from the group consisting of lithium, sodium, potassium, rubidium and cesium compounds.
[0035] According to the present invention, preferably, in step (4), the alkaline earth metal additive is selected from at least one of oxides, oxalates, sulfates, acetates and nitrates of alkaline earth metal elements.
[0036] According to the present invention, preferably, in step (4), the rhenium auxiliary agent is selected from at least one of rhenium oxide, perrhenic acid and perrhenate.
[0037] According to the present invention, preferably, in step (4), the rhenium co-promoter is selected from at least one of chromium, molybdenum, tungsten, boron, chromium metal compounds, molybdenum metal compounds, tungsten metal compounds and boron compounds.
[0038] According to the present invention, preferably, in step (4), based on the total weight of the impregnation solution, the content of the silver-containing compound in the impregnation solution in terms of silver element is 5-40wt%, the content of the organic amine is 10-90wt%, preferably 10-60wt%, the content of the alkali metal additive is 5-2000ppm, the content of the alkaline earth metal additive is 5-8000ppm, the content of the rhenium additive is 0-5000ppm, preferably 5-5000ppm, the content of the rhenium co-additive is 0-5000ppm, preferably 5-5000ppm, the content of the water is 0.1-60wt%, preferably 20-60wt%, and more preferably 30-50wt%.
[0039] According to the present invention, preferably, in step (5), the weight ratio of the impregnation liquid to the substrate is 10 to 30:1.
[0040] According to the present invention, preferably, in step (5), the immersion is carried out at a pressure below 100 mmHg, at a temperature below 30° C., and for a time of 10 to 300 min.
[0041] According to the present invention, preferably, in step (5), the activation is carried out under flowing air and / or inert gas atmosphere, the activation temperature is 120 to 480° C., and the activation time is 0.3 to 150 min.
[0042] Another object of the present invention is to provide a regenerated silver catalyst obtained by the regeneration method.
[0043] The present invention also provides an application of the regenerated silver catalyst in preparing ethylene oxide by ethylene oxidation.
[0044] The present invention will be further described below in conjunction with embodiments, but the scope of the present invention is not limited to these embodiments.
[0045] Determination of catalyst performance:
[0046] The various silver catalysts of the present invention are tested for their initial performance and stability using a laboratory reactor (hereinafter referred to as "micro-reactor") evaluation device. The reactor used in the micro-reactor evaluation device is a stainless steel tube with an inner diameter of 4 mm, and the reactor is placed in a heating jacket. The catalyst loading volume is 1 mL, and there is an inert filler at the bottom, so that the catalyst bed is located in the constant temperature zone of the heating jacket.
[0047] The activity and selectivity determination conditions used in the present invention are as follows:
[0048] Reaction gas composition (mol%)
[0049]
[0050] When the above reaction conditions are stably reached, the gas composition at the reactor inlet and outlet is continuously measured. The selectivity is calculated according to the following formula after volume shrinkage correction is performed on the measured results:
[0051]
[0052] Where ΔEO is the difference in ethylene oxide concentration between the outlet gas and the inlet gas, ΔCO2 is the difference in carbon dioxide concentration between the outlet gas and the inlet gas of the reactor, and the average of more than 10 groups of test data is taken as the test result of the day.
[0053] The present invention is further described in conjunction with the following examples, but the scope of the present invention is not limited to these examples.
[0054] Comparative Example 1
[0055] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0056] (1) 20 g of YS-8520G silver catalyst (medium-high selectivity silver catalyst) which was used in an EOEG device of a certain factory for 3 years and then removed was added to 100 g of deionized water to obtain a solid-liquid mixture;
[0057] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 200 W ultrasonic cleaning machine at room temperature for 10 min;
[0058] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 6 minutes at a speed of 4000 rpm;
[0059] (4) The solid obtained by centrifugation in step (3) was placed in an oven at 120° C. and dried for 6 h to obtain a regenerated silver catalyst.
[0060] Comparative Example 2
[0061] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0062] (1) 20 g of YS-8520G silver catalyst (medium-high selectivity silver catalyst) which was used in an EOEG device of a certain factory for 3 years and then removed was added to 100 g of methanol to obtain a solid-liquid mixture;
[0063] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 200 W ultrasonic cleaning machine at room temperature for 10 min;
[0064] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 10 min at a speed of 4000 rpm;
[0065] (4) The solid obtained by centrifugation in step (3) was placed in an oven at 100° C. and dried for 4 h to obtain a regenerated silver catalyst.
[0066] Comparative Example 3
[0067] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0068] (1) Take 20g of YS-8520G silver catalyst (medium-high selectivity silver catalyst) which was removed from the EOEG device of a certain factory after being used for 3 years and set aside;
[0069] (2) 50 g of ethylamine, 20 g of ethanolamine, and 100 g of deionized water were mixed evenly and cooled in a water bath to 20° C., 50 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.40 g of cesium nitrate, 0.60 g of strontium acetate, 0.39 g of ammonium perrhenate, and 0.20 g of potassium nitrate were added thereto, mixed evenly, and used as an impregnation solution for later use;
[0070] (3) The silver catalyst in step (1) is impregnated with the impregnation solution in step (2), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the catalyst is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0071] Example 1
[0072] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0073] (1) 20 g of YS-8520G silver catalyst (medium-high selectivity silver catalyst) which was used in an EOEG device of a certain factory for 3 years and then removed was added to 100 g of methanol to obtain a solid-liquid mixture;
[0074] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 200 W ultrasonic cleaning machine at room temperature for 10 min;
[0075] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 8 minutes at a speed of 4000 rpm;
[0076] (4) drying the solid obtained by centrifugation in step (3) in an oven at 120° C. for 6 h to obtain a substrate;
[0077] (5) 50 g of ethylamine, 20 g of ethanolamine, and 100 g of deionized water were mixed uniformly and cooled in a water bath to 20° C., 50 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.40 g of cesium nitrate, 0.60 g of strontium acetate, 0.39 g of ammonium perrhenate, and 0.20 g of potassium nitrate were added thereto, mixed uniformly, and used as an impregnation solution for later use;
[0078] (6) The substrate in step (4) is impregnated with the impregnation solution in step (5), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the substrate is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0079] Example 2
[0080] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0081] (1) 20 g of YS-8520G silver catalyst (medium-high selectivity silver catalyst) which was used in an EOEG device of a certain factory for 3 years and then removed was added to 100 g of deionized water to obtain a solid-liquid mixture;
[0082] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment at room temperature for 15 min in a 350 W ultrasonic cleaning machine;
[0083] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 6 minutes at a speed of 4500 rpm;
[0084] (4) drying the solid obtained by centrifugation in step (3) in an oven at 130° C. for 5 h to obtain a substrate;
[0085] (5) 50 g of ethylamine, 20 g of ethanolamine, and 100 g of deionized water were mixed uniformly and cooled in a water bath to 20° C., 50 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.50 g of cesium nitrate, 0.63 g of strontium acetate, 0.39 g of ammonium perrhenate, and 0.30 g of potassium nitrate were added thereto, mixed uniformly, and used as an impregnation solution for later use;
[0086] (6) The substrate in step (4) is impregnated with the impregnation solution in step (5), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the substrate is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0087] Example 3
[0088] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0089] (1) 20 g of the YS-8520 silver catalyst (medium-high selectivity silver catalyst) unloaded after 2.5 years of evaluation in a fixed bed reactor was added to 100 g of n-hexane to obtain a solid-liquid mixture;
[0090] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 200 W ultrasonic cleaning machine at room temperature for 12 min;
[0091] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 8 minutes at a speed of 4000 rpm;
[0092] (4) drying the solid obtained by centrifugation in step (3) in an oven at 120° C. for 5 h to obtain a substrate;
[0093] (5) 45 g of ethylamine, 25 g of ethanolamine, and 100 g of deionized water were mixed uniformly and cooled in a water bath to 20° C., 45 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.650 g of cesium nitrate, 0.72 g of strontium acetate, 0.53 g of ammonium perrhenate, and 0.46 g of potassium nitrate were added thereto, mixed uniformly, and used as an impregnation solution for later use;
[0094] (6) The substrate in step (4) is impregnated with the impregnation solution in step (5), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the substrate is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0095] Example 4
[0096] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0097] (1) 20 g of YS-8520H silver catalyst (medium-high selectivity silver catalyst) removed from the fixed bed reactor after evaluation for 2.5 years was added to 100 g of ethanol to obtain a solid-liquid mixture;
[0098] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 300 W ultrasonic cleaning machine at room temperature for 12 min;
[0099] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 6 minutes at a speed of 4800 rpm;
[0100] (4) drying the solid obtained by centrifugation in step (3) in an oven at 110° C. for 7 h to obtain a substrate;
[0101] (5) 48 g of ethylamine, 22 g of ethanolamine, and 100 g of deionized water were mixed uniformly and cooled in a water bath to 20° C., 45 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.60 g of cesium nitrate, 0.70 g of strontium acetate, 0.43 g of ammonium perrhenate, and 0.40 g of potassium nitrate were added thereto, mixed uniformly, and used as an impregnation solution for later use;
[0102] (6) The substrate in step (4) is impregnated with the impregnation solution in step (5), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the substrate is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0103] Example 5
[0104] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0105] (1) 20 g of YS-8520G silver catalyst (medium-high selectivity silver catalyst) which was used in an EOEG device of a certain factory for 3 years and then removed was added to 100 g of cyclohexane to obtain a solid-liquid mixture;
[0106] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 400 W ultrasonic cleaning machine at room temperature for 12 min;
[0107] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 8 minutes at a speed of 4000 rpm;
[0108] (4) drying the solid obtained by centrifugation in step (3) in an oven at 120° C. for 5 h to obtain a substrate;
[0109] (5) 50 g of ethylamine, 20 g of ethanolamine, and 100 g of deionized water were mixed uniformly and cooled in a water bath to 20° C., 50 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.50 g of cesium nitrate, 0.60 g of strontium acetate, 0.80 g of ammonium perrhenate, and 0.20 g of potassium nitrate were added thereto, mixed uniformly, and used as an impregnation solution for later use;
[0110] (6) The substrate in step (4) is impregnated with the impregnation solution in step (5), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the substrate is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0111] Example 6
[0112] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0113] (1) 20 g of YS-7 silver catalyst (high-activity silver catalyst) which was used in an EOEG device of a certain factory for 3 years and then removed was added to 100 g of methanol to obtain a solid-liquid mixture;
[0114] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 200 W ultrasonic cleaning machine at room temperature for 10 min;
[0115] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 8 minutes at a speed of 4000 rpm;
[0116] (4) drying the solid obtained by centrifugation in step (3) in an oven at 120° C. for 6 h to obtain a substrate;
[0117] (5) 50 g of ethylamine, 20 g of ethanolamine, and 100 g of deionized water were mixed uniformly and cooled in a water bath to 20° C., 50 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.40 g of cesium nitrate, 0.60 g of strontium acetate, 0.39 g of ammonium perrhenate, and 0.20 g of potassium nitrate were added thereto, mixed uniformly, and used as an impregnation solution for later use;
[0118] (6) The substrate in step (4) is impregnated with the impregnation solution in step (5), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the substrate is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0119] Example 7
[0120] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0121] (1) 20 g of YS-8520G silver catalyst (medium-high selectivity silver catalyst) which was used in an EOEG device of a certain factory for 3 years and then removed was added to 100 g of methanol to obtain a solid-liquid mixture;
[0122] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 1000 W ultrasonic cleaning machine at room temperature for 30 min;
[0123] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 8 minutes at a speed of 4000 rpm;
[0124] (4) drying the solid obtained by centrifugation in step (3) in an oven at 120° C. for 6 h to obtain a substrate;
[0125] (5) 50 g of ethylamine, 20 g of ethanolamine, and 100 g of deionized water were mixed uniformly and cooled in a water bath to 20° C., 50 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.40 g of cesium nitrate, 0.60 g of strontium acetate, 0.39 g of ammonium perrhenate, and 0.20 g of potassium nitrate were added thereto, mixed uniformly, and used as an impregnation solution for later use;
[0126] (6) The substrate in step (4) is impregnated with the impregnation solution in step (5), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the substrate is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0127] Example 8
[0128] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0129] (1) 20 g of YS-8520G (medium-high selectivity silver catalyst) silver catalyst which was used in an EOEG device of a certain factory for 3 years and then removed was added to 100 g of methanol to obtain a solid-liquid mixture;
[0130] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 50W ultrasonic cleaning machine at room temperature for 1 min;
[0131] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 8 minutes at a speed of 4000 rpm;
[0132] (4) drying the solid obtained by centrifugation in step (3) in an oven at 120° C. for 6 h to obtain a substrate;
[0133] (5) 50 g of ethylamine, 20 g of ethanolamine, and 100 g of deionized water were mixed uniformly and cooled in a water bath to 20° C., 50 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.40 g of cesium nitrate, 0.60 g of strontium acetate, 0.39 g of ammonium perrhenate, and 0.20 g of potassium nitrate were added thereto, mixed uniformly, and used as an impregnation solution for later use;
[0134] (6) The substrate in step (4) is impregnated with the impregnation solution in step (5), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the substrate is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0135] Example 9
[0136] The present invention provides a method for regenerating a waste silver catalyst for preparing ethylene oxide by ethylene oxidation, comprising the following steps:
[0137] (1) 20 g of YS-8520G silver catalyst (medium-high selectivity silver catalyst) which was used in an EOEG device of a certain factory for 3 years and then removed was added to 100 g of hexanol to obtain a solid-liquid mixture;
[0138] (2) treating the solid-liquid mixture in step (1) by ultrasonic treatment in a 200 W ultrasonic cleaning machine at room temperature for 10 min;
[0139] (3) treating the solid-liquid mixture after ultrasonic treatment in step (2) in a centrifuge for 8 minutes at a speed of 4000 rpm;
[0140] (4) drying the solid obtained by centrifugation in step (3) in an oven at 120° C. for 6 h to obtain a substrate;
[0141] (5) 50 g of ethylamine, 20 g of ethanolamine, and 100 g of deionized water were mixed uniformly and cooled in a water bath to 20° C., 50 g of silver acetate was slowly added thereto, and after the silver acetate was completely dissolved, 0.40 g of cesium nitrate, 0.60 g of strontium acetate, 0.39 g of ammonium perrhenate, and 0.20 g of potassium nitrate were added thereto, mixed uniformly, and used as an impregnation solution for later use;
[0142] (6) The substrate in step (4) is impregnated with the impregnation solution in step (5), and the pressure is reduced to below 10 mmHg by vacuuming. After impregnation for half an hour, the substrate is taken out, filtered, and activated in air at 300° C. to obtain a regenerated silver catalyst.
[0143] Test Case
[0144] The reaction characteristics of the catalyst samples were measured under the aforementioned process conditions using a microreactor evaluation device. Each sample was evaluated for one month after the process conditions were stabilized, and the silver content was determined by chemical titration. The test results are listed in Table 1.
[0145] Table 1 Catalytic performance of each regenerated silver catalyst
[0146]
[0147]
[0148] By comparing the data in Table 1, it can be seen that compared with the regenerated catalyst prepared by only using an inert organic solvent and / or water treatment and only secondary impregnation activation, the activity and selectivity of the regenerated catalyst prepared by first using an organic solvent and / or water treatment and then continuing to use secondary impregnation activation are significantly improved, which shows that medium-to-high selectivity and high-activity waste silver catalysts can be regenerated into high-selectivity silver catalysts.
[0149] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0150] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A method for regenerating a spent silver catalyst for preparing ethylene oxide by ethylene oxidation, It is characterized in that The steps include: (1) adding a waste silver catalyst for preparing ethylene oxide by oxidation of ethylene to a solvent to obtain a solid-liquid mixture; the solvent is an inert organic solvent and / or water; (2) subjecting the solid-liquid mixture obtained in step (1) to ultrasonic treatment to obtain an ultrasonically treated solid-liquid mixture; (3) centrifuging and drying the solid-liquid mixture after ultrasonic treatment obtained in step (2) to obtain a substrate; (4) obtaining an impregnation solution comprising a silver-containing compound, an organic amine, water, an alkali metal additive, an alkaline earth metal additive, an optional rhenium additive and a co-additive thereof; (5) The substrate obtained in step (3) is impregnated with the impregnation solution in step (4), and then activated by leaching to obtain a regenerated silver catalyst.
2. The regeneration method according to claim 1, in, In step (1), the mass ratio of the solvent to the waste silver catalyst for preparing ethylene oxide by ethylene oxidation is 1 to 20:1, preferably 1.5 to 15:1, and more preferably 2 to 10:
1.
3. The regeneration method according to claim 1, in, In step (1), the waste silver catalyst for ethylene oxidation to ethylene oxide is a silver catalyst for ethylene oxidation to ethylene oxide at the end of the reaction, preferably a medium-high selectivity silver catalyst or a high-activity silver catalyst at the end of the reaction, and more preferably a medium-high selectivity silver catalyst or a high-activity silver catalyst with a reaction temperature higher than 250°C.
4. The regeneration method according to claim 1, in, In step (1), the inert organic solvent is selected from at least one of C1-C6 fatty alcohols, C6-C8 fatty hydrocarbons and C6-C8 alicyclic hydrocarbons, preferably selected from at least one of methanol, ethanol, isopropanol, n-hexane and cyclohexane; and the water is deionized water.
5. The regeneration method according to claim 1, in, In step (2), the ultrasonic treatment is carried out in an ultrasonic device; preferably, the ultrasonic device is an ultrasonic cleaning machine, the power of the ultrasonic treatment is 35 to 18000 W, preferably 100 to 500 W, the temperature is 10 to 80° C., and the time is 0.1 to 99 min, preferably 5 to 20 min.
6. The regeneration method according to claim 1, in, In step (3), the centrifugal treatment is carried out in a centrifuge. Preferably, the rotation speed of the centrifugal treatment is 100 to 16500 rpm and the time is 1 to 100 min.
7. The regeneration method according to claim 1, in, In step (3), the drying temperature is 30 to 150° C. and the drying time is 0.1 to 10 h.
8. The regeneration method according to claim 1, in, In step (4), the silver-containing compound is selected from at least one of silver nitrate, silver acetate and silver oxalate; The organic amine is selected from at least one of ethylamine, ethylenediamine, n-propylamine, 1,3-propylenediamine, n-butylamine, 1,4-butylenediamine, ethanolamine and propanolamine; The alkali metal auxiliary agent is selected from at least one of lithium, sodium, potassium, rubidium and cesium compounds; The alkaline earth metal additive is selected from at least one of oxides, oxalates, sulfates, acetates and nitrates of alkaline earth metal elements; The rhenium auxiliary agent is selected from at least one of rhenium oxide, perrhenic acid and perrhenate; The rhenium co-promoter is selected from at least one of chromium, molybdenum, tungsten, boron, chromium metal compounds, molybdenum metal compounds, tungsten metal compounds and boron compounds; Based on the total weight of the impregnation solution, the content of the silver-containing compound in the impregnation solution in terms of silver element is 5 to 40 wt %, the content of the organic amine is 10 to 90 wt %, the content of the alkali metal additive is 5 to 2000 ppm, the content of the alkaline earth metal additive is 5 to 8000 ppm, the content of the rhenium additive is 0 to 5000 ppm, preferably 5 to 5000 ppm, the content of the rhenium co-additive is 0 to 5000 ppm, preferably 5 to 5000 ppm, and the content of water is 0.1 to 60 wt %, preferably 20 to 60 wt %, and more preferably 30 to 50 wt %.
9. The regeneration method according to claim 1, in, In step (5), the weight ratio of the impregnation liquid to the substrate is 10 to 30:
1.
10. The regeneration method according to claim 1, in, In step (5), the immersion is carried out at a pressure below 100 mmHg, a temperature below 30° C., and a time of 10 to 300 min.
11. The regeneration method according to claim 1, in, In step (5), the activation is carried out in a flowing air and / or inert gas atmosphere, the activation temperature is 120 to 480° C., and the activation time is 0.3 to 150 min.
12. A regenerated silver catalyst obtained by the regeneration method according to any one of claims 1 to 11.
13. Use of the regenerated silver catalyst according to claim 12 in preparing ethylene oxide by oxidation of ethylene.
Citation Information
Patent Citations
Preparation method of silver catalyst for producing ethylene oxide, silver catalyst prepared thereby and application thereof
CN102527384A