Silicon wafer cleaning and recycling method
Through the combined treatment of high-concentration sulfuric acid and alkaline cleaning fluid, the problem of recycling silicon wafers after exposure is solved, effective cleaning and reuse of silicon wafers is achieved, and resource waste and production costs are reduced.
Patent Information
- Application Number
- CN202410792093.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-01
AI Technical Summary
There is a lack of effective methods in the existing technology to recycle and reuse exposed silicon wafers, resulting in resource waste and increased production costs.
A silicon wafer cleaning and recycling method is adopted, which includes soaking the silicon wafer in an acidic cleaning solution of high-concentration sulfuric acid and hydrogen peroxide, and then processing it in an alkaline ammonia and hydrogen peroxide cleaning solution to remove BARC and photoresist on the surface , maintaining the original characteristics of the silicon wafer.
It effectively removes BARC and photoresist on the exposed silicon wafer, keeping the surface of the silicon wafer smooth and pollution-free, realizing the recycling and reuse of silicon wafers, reducing resource waste and production costs, and the operation is simple and does not require expensive instruments.
Smart Images

Figure CN118719682A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductors, and in particular relates to a method for cleaning and recycling a silicon wafer. Background Art
[0002] Silicon wafers are thin slices grown from high-purity silicon crystals, usually in a round shape. As the basis of semiconductor materials, they are the substrates for manufacturing various electronic components (such as transistors and integrated circuits). Silicon wafers are the raw material state of wafers and are the basic form before subsequent semiconductor manufacturing.
[0003] Silicon wafers are the main substrate of chips. They are made from high-purity polycrystalline silicon or single crystal silicon rods through steps such as crystal pulling, cutting, grinding and polishing, and cleaning. The production cost is high. Usually for photoresist research and development companies, these discarded silicon wafers also lead to a significant increase in semiconductor research and development or manufacturing costs and waste of resources.
[0004] In addition, with the rapid development of the semiconductor industry, more and more companies and research institutions are investing in semiconductor manufacturing and research. The semiconductor manufacturing process includes steps such as wafer processing, photolithography, etching, and deposition. The photolithography process steps include: coating bottom anti-reflective coating (BARC, optional steps according to demand), coating photoresist, exposure, and development. In the research of photolithography or the manufacturing process of semiconductors, there will be a large number of unqualified exposed silicon wafers or discarded silicon wafers. If these silicon wafers are not recycled and treated as waste, a large amount of waste will be generated. From the perspective of cost saving, recycling and reusing the above silicon wafers is a relatively economical disposal method. Summary of the invention
[0005] There is no related report on the recycling of exposed silicon wafers. In view of the above-mentioned problem of discarded exposed silicon wafers, the present invention provides a method for cleaning and recycling silicon wafers. The recycling method can effectively remove the BARC and photoresist coated on the exposed silicon wafers, while keeping the properties of the silicon wafers unchanged, so that the silicon wafers can be reused for exposure and development.
[0006] A method for cleaning and recycling a silicon wafer, the method comprising:
[0007] S1. Place the silicon wafer to be cleaned in an acidic cleaning solution and soak it at 100°C or above for 10-60 minutes;
[0008] S2. After soaking in the acid cleaning solution, washing with water to remove the residual acid cleaning solution on the surface of the silicon wafer;
[0009] S3, placing the silicon wafer in an alkaline cleaning solution for a soaking time of 10 min to 20 min, preferably 10 min to 12 min;
[0010] S4, after soaking in the alkaline cleaning solution, washing with water to remove the alkaline cleaning solution remaining on the surface of the silicon wafer, and drying for later use;
[0011] The surface of the silicon wafer to be cleaned is coated with a bottom anti-reflective coating and a photoresist and is subjected to exposure and development treatment;
[0012] The acid cleaning solution comprises: sulfuric acid and hydrogen peroxide, wherein the content of sulfuric acid is higher than 80%;
[0013] The alkaline cleaning solution comprises: ammonia water and hydrogen peroxide, wherein the content of the ammonia water is 5%-20%, and the content of the hydrogen peroxide is 5%-20%.
[0014] In some embodiments, the acid cleaning solution is composed of sulfuric acid, hydrogen peroxide and water, and the content of hydrogen peroxide is 5% to 15%.
[0015] In some embodiments, the alkaline cleaning solution is composed of ammonia water, hydrogen peroxide and water, the content of ammonia water is 5% to 15%, and the content of hydrogen peroxide is 10% to 15%.
[0016] In some embodiments, the step S1 is performed by soaking at 105° C.-135° C. for 10 min-60 min.
[0017] In some embodiments, the temperature of water in step S2 is 40°C-60°C.
[0018] In some embodiments, hot nitrogen is used for drying in step S4.
[0019] In some embodiments, the silicon wafer to be cleaned is a 12-inch wafer.
[0020] In some embodiments, the photoresist is a 193 nm photoresist (containing methacrylate resin), preferably ArF photoresist.
[0021] In some embodiments, the photoresist has a thickness of 1000 angstroms to 2000 angstroms.
[0022] In some embodiments, the acidic cleaning solution in step S1 can be reused, and cannot be used when the acidic cleaning solution turns dark brown.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] There is no related report on recycling silicon wafers after exposure in the current technology. The method of the present invention can clean and remove the BARC and / or photoresist coated on the silicon wafer after exposure and before etching, while maintaining the original properties of the silicon wafer surface, and can be reused as a substrate for semiconductor manufacturing and research. In this way, the discarded silicon wafer after exposure can be recycled and reused, avoiding waste of resources and reducing the R&D or production costs of enterprises. At the same time, the method of the present invention is simple to operate and does not require expensive instruments, and is particularly suitable for laboratory research and development. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of a silicon wafer containing a BARC layer and a photoresist layer after exposure according to the present invention;
[0026] Figure 2 Schematic diagram of a silicon wafer containing a photoresist layer after exposure according to the present invention;
[0027] Figure 3 Example 1: Photo of silicon wafer after cleaning;
[0028] Figure 4 Example 2: Photo of silicon wafer after cleaning;
[0029] Figure 5 Example 3: Photo of silicon wafer after cleaning;
[0030] Figure 6 Example 4: Photo of silicon wafer after cleaning;
[0031] Figure 7 Comparative Example 1: Image of silicon wafer after cleaning;
[0032] Figure 8 Comparative Example 2: Silicon wafer image after cleaning;
[0033] Fig. 9 Comparative Example 3: Image of silicon wafer after cleaning;
[0034] Fig.10 Comparative Example 4: Image of silicon wafer after cleaning;
[0035] In the figure, 1 is the silicon wafer base layer, 2 is the oxide film, 3 is BARC, and 4 is the photoresist. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0037] The cleaning process in the existing semiconductor process includes pre-wafer (substrate material) cleaning and post-etching cleaning. The purpose of pre-wafer cleaning is to remove impurities on the surface of the wafer, including organic substances such as grease, rosin, wax, epoxy resin, polyethylene glycol, metals, metal ions and some inorganic compounds, dust and other particles. These impurities can be removed by RCA cleaning method and improved method. For example, CN116631848A adds a step of using SC1 cleaning solution with chelating agent to clean on the basis of RCA cleaning method, which can solve the particle contamination problem caused by SC2 cleaning. In addition, there are other new cleaning methods, such as ozone cleaning in CN 111151489 A. Post-etching cleaning is to clean and remove the photoresist and polymer residues after etching. CN 111045300 A uses O2 / CF4 mixed gas to remove SU-8 negative photoresist by plasma etching with wet method. This method is only applicable to specific photoresists and has a narrow application range. In addition, CF4 in it will damage the silicon wafer substrate.
[0038] Different from the above-mentioned pre-wafer cleaning and post-etching cleaning, the method of the present invention is used for cleaning the silicon wafer after exposure and before etching, with the purpose of removing the photoresist and other impurities on the surface of the silicon wafer. Figure 1 As shown, the exposed silicon wafer includes: a silicon wafer layer 1, an oxide film 2, a BARC 3 and a photoresist layer 4, or as shown in FIG. Figure 2 As shown, after exposure, the silicon wafer may be free of a BARC layer, that is, it includes in sequence: a silicon wafer layer 1, an oxide film 2 and a photoresist layer 4. The method of the present invention can remove the BARC 3 and / or the photoresist layer 4, and form a new oxide film 2, thereby realizing the recycling and reuse of these two types of silicon wafers.
[0039] A method for cleaning and recycling a silicon wafer of the present invention comprises the following steps:
[0040] S1. Place the silicon wafer to be cleaned in an acidic cleaning solution and soak it at 105°C or above for 10-60 minutes;
[0041] S2. After soaking in the acid cleaning solution, washing with water to remove the residual acid cleaning solution on the surface of the silicon wafer;
[0042] S3, placing the silicon wafer in an alkaline cleaning solution and soaking for 10-20 minutes;
[0043] S4, after soaking in the alkaline cleaning solution, washing with water to remove the alkaline cleaning solution remaining on the surface of the silicon wafer, and drying for later use;
[0044] The surface of the silicon wafer to be cleaned is coated with a bottom anti-reflective coating and a photoresist and is exposed;
[0045] The acid cleaning solution comprises: sulfuric acid and hydrogen peroxide, wherein the content of sulfuric acid is higher than 80%;
[0046] The alkaline cleaning solution comprises: ammonia water and hydrogen peroxide, wherein the content of the ammonia water is 5.0%-15.0%, and the content of the hydrogen peroxide is 5.0%-15.0%.
[0047] The acidic cleaning solution contains high concentrations of sulfuric acid and hydrogen peroxide, which can oxidize and decompose the photoresist layer 4 on the surface of the silicon wafer to be cleaned, and then dissolve and remove it. At the same time, the BARC 3 at the bottom can be further removed under heating conditions (105°C). Then, an alkaline cleaning solution containing ammonia and hydrogen peroxide is used to further react with the oxide film 2 on the surface of the silicon wafer, thereby causing a small amount of BARC or photoresist that may remain on the surface to fall off, and at the same time, a new oxide film is formed on the surface of the silicon wafer. Finally, the method of the present invention can effectively remove the exposed photoresist and the bottom BARC without affecting the silicon wafer, so that the surface of the silicon wafer is free of pollutants and is smooth and flat, and the subsequent BARC and / or photoresist coating operations can be directly carried out.
[0048] Embodiment 1
[0049] The structure of the silicon wafer to be cleaned is as follows Figure 1 As shown, the 12-inch wafer was discarded after the company conducted photolithography process research. It was coated with a BARC layer (about 900 angstroms thick) and an ArF photoresist (about 1000 angstroms thick) and was exposed and developed. The cleaning and recycling method is as follows: Steps 1-9:
[0050] 1. Place 12 silicon wafers to be washed in a silicon wafer basket for later use.
[0051] 2. Prepare the acidic cleaning solution in cleaning tank 1: transfer 50L of sulfuric acid (98%) and 10L of hydrogen peroxide (31%) to cleaning tank 1, heat and circulate and filter to 105°C.
[0052] 3. When the temperature of the acid cleaning solution in cleaning tank 1 reaches 105°C, carefully place the flower basket in 1 into the acid cleaning solution and soak for about 30 minutes.
[0053] 4. After soaking, transfer the flower basket to a hot water tank and rinse and soak for 10 minutes.
[0054] 5. Prepare alkaline cleaning solution in cleaning tank 2: transfer 5L ammonia water (30%), 10L hydrogen peroxide (31%) and 50L pure water to cleaning tank 2.
[0055] 6. Transfer the flower basket in step 4 to cleaning tank 2 and perform ultrasonic cleaning for 10 minutes.
[0056] 7. Transfer the flower basket to the sink and rinse it. Soak it in pure water 3 times.
[0057] 8. After completion, transfer the flower basket to the drying tank for hot nitrogen drying (hot nitrogen temperature is 60℃ and dried for 20 minutes).
[0058] 9. After drying, the silicon wafer is transferred to a silicon wafer box in a clean environment for glue coating.
[0059] Results: Figure 3 The cleaning effectively removes the BARC and photoresist layers on the surface, and the surface of the silicon wafer is smooth, free of pollutants, and like a mirror.
[0060] Each batch of 12 silicon wafers to be cleaned is cleaned, and the acid cleaning solution in the cleaning tank 1 can clean 45 batches. After cleaning 45 batches, the color of the acid cleaning solution turns dark brown and has a strong odor. The cleaning effect is not good and it can no longer be used.
[0061] Embodiment 2
[0062] The structure of the silicon wafer to be cleaned is as follows Figure 2 As shown, the 12-inch wafer is discarded after the company's photolithography process research. ArF photoresist (about 2000 angstroms thick) is coated on it and exposed and developed. The cleaning and recycling method is as follows: Steps 1-9:
[0063] 1. Place 12 silicon wafers to be washed in a silicon wafer basket for later use.
[0064] 2. Prepare the acid cleaning solution in cleaning tank 1: transfer 50L sulfuric acid (98%) and 10L hydrogen peroxide (31%) to cleaning tank 1, heat and circulate and filter to 100°C.
[0065] 3. After the temperature of the acid cleaning solution in cleaning tank 1 reaches 120°C, carefully place the flower basket in 1 into the acid cleaning solution and soak for about 30 minutes.
[0066] 4. After soaking, transfer the flower basket to a hot water tank and rinse and soak for 10 minutes.
[0067] 5. Prepare alkaline cleaning solution in cleaning tank 2: transfer 5L of ammonia water (30%), 10L of hydrogen peroxide (31%) and 50L of pure water to cleaning tank 2.
[0068] 6. Transfer the flower basket in step 4 to cleaning tank 2 and perform ultrasonic cleaning for 10 minutes.
[0069] 7. Transfer the flower basket to the sink and rinse it. Soak it in pure water 3 times.
[0070] 8. After completion, transfer the flower basket to the drying tank for hot nitrogen drying (hot nitrogen temperature is 60℃ and dried for 20 minutes).
[0071] 9. After drying, the silicon wafer is transferred to a silicon wafer box in a clean environment for glue coating.
[0072] Results: Figure 4The cleaning effectively removes the photoresist layer on the surface, and the surface of the silicon wafer is smooth with no pollutants remaining.
[0073] Each batch of 12 silicon wafers to be cleaned is cleaned, and the acid cleaning solution in the cleaning tank 1 can clean 36 batches. After cleaning 36 batches, the acid cleaning solution turns dark brown and has a strong odor, and the cleaning effect is poor, so it can no longer be used.
[0074] Embodiment 3
[0075] The structure of the silicon wafer to be cleaned is as follows Figure 1 As shown, the 12-inch wafer is discarded after the company conducted photolithography process research. It is coated with a BARC layer (about 1000 angstroms thick) and an ArF photoresist (about 2000 angstroms thick) and has been exposed and developed. The cleaning and recycling method is as follows: Steps 1-9:
[0076] 1. Place 12 silicon wafers to be washed in a silicon wafer basket for later use;
[0077] 2. Prepare the acidic cleaning solution in cleaning tank 1: transfer 50L of sulfuric acid (98%) and 10L of hydrogen peroxide (31%) to cleaning tank 1, heat and circulate and filter to 130°C.
[0078] 3. After the temperature of the acid cleaning solution in the cleaning tank 1 reaches 130°C, carefully place the flower basket in 1 into the heated acid cleaning solution and soak for about 30 minutes;
[0079] 4. After soaking, transfer the flower basket to a hot water tank and rinse and soak for 10 minutes.
[0080] 5. Prepare alkaline cleaning solution in cleaning tank 2: transfer 5L of ammonia water (30%), 10L of hydrogen peroxide (31%) and 50L of pure water to cleaning tank 2.
[0081] 6. Transfer the flower basket in step 4 to cleaning tank 2 and perform ultrasonic cleaning for 10 minutes.
[0082] 7. Transfer the flower basket to the sink and rinse it. Soak it in pure water 3 times.
[0083] 8. After completion, transfer the flower basket to the drying tank for hot nitrogen drying (hot nitrogen temperature is 60℃ and dried for 20 minutes).
[0084] 9. After drying, the silicon wafer is transferred to a silicon wafer box in a clean environment for glue coating.
[0085] Results: Figure 5 The cleaning effectively removes the BARC and photoresist layers on the surface, leaving the silicon wafer surface smooth and free of contaminants.
[0086] Each batch of 12 silicon wafers to be cleaned is cleaned, and the acid cleaning solution in the cleaning tank 1 can clean 85 batches. After cleaning 85 batches, the acid cleaning solution turns dark brown and has a strong odor, and the cleaning effect is poor, so it can no longer be used.
[0087] Embodiment 4
[0088] The structure of the silicon wafer to be cleaned is as follows Figure 1 As shown, the 12-inch wafer is discarded after the company conducted photolithography process research. It is coated with a BARC layer (about 1000 angstroms thick) and an ArF photoresist (about 2000 angstroms thick) and has been exposed and developed. The cleaning and recycling method is as follows: Steps 1-9:
[0089] 1. Place 12 silicon wafers to be washed in a silicon wafer basket for later use;
[0090] 2. Prepare the acidic cleaning solution in cleaning tank 1: transfer 50L of sulfuric acid (98%) and 10L of hydrogen peroxide (31%) to cleaning tank 1, heat and circulate and filter to 135°C.
[0091] 3. After the temperature of the acid cleaning solution in the cleaning tank 1 reaches 135°C, carefully place the flower basket in 1 into the heated acid cleaning solution and soak for about 30 minutes;
[0092] 4. After soaking, transfer the flower basket to a hot water tank and rinse and soak for 10 minutes.
[0093] 5. Prepare alkaline cleaning solution in cleaning tank 2: transfer 5L of ammonia water (30%), 10L of hydrogen peroxide (31%) and 50L of pure water to cleaning tank 2.
[0094] 6. Transfer the flower basket in step 4 to cleaning tank 2 and perform ultrasonic cleaning for 10 minutes.
[0095] 7. Transfer the flower basket to the sink and rinse it. Soak it in pure water 3 times.
[0096] 8. After completion, transfer the flower basket to the drying tank for hot nitrogen drying (hot nitrogen temperature is 60℃ and dried for 20 minutes).
[0097] 9. After drying, the silicon wafer is transferred to a silicon wafer box in a clean environment for glue coating.
[0098] Results: Figure 6 The cleaning effectively removes the BARC and photoresist layers on the surface, leaving the silicon wafer surface smooth and free of contaminants.
[0099] Each batch of 12 silicon wafers to be cleaned is cleaned, and the acid cleaning solution in the cleaning tank 1 can clean 85 batches. After cleaning 85 batches, the acid cleaning solution turns dark brown and has a strong odor, and the cleaning effect is poor, so it can no longer be used.
[0100] Comparative Example 1
[0101] The structure of the silicon wafer to be cleaned is as follows Figure 1 As shown, the 12-inch wafer was discarded after the company conducted photolithography process research. It was coated with a BARC layer (about 900 angstroms thick) and an ArF photoresist (about 1000 angstroms thick) and was exposed and developed. The cleaning and recycling method is as follows: Steps 1-9:
[0102] 1. Place 12 silicon wafers to be washed in a silicon wafer basket for later use.
[0103] 2. Prepare the acidic cleaning solution in cleaning tank 1: transfer 50L nitric acid (≥90%) and 10L hydrogen peroxide (31%) to cleaning tank 1, heat and circulate and filter to 105°C.
[0104] 3. When the temperature of the acid cleaning solution in cleaning tank 1 reaches 105°C, carefully place the flower basket in 1 into the acid cleaning solution and soak for about 30 minutes.
[0105] 4. After soaking, transfer the flower basket to a hot water tank and rinse and soak for 10 minutes.
[0106] 5. Prepare alkaline cleaning solution in cleaning tank 2: transfer 5L ammonia water (30%), 10L hydrogen peroxide (31%) and 50L pure water to cleaning tank 2.
[0107] 6. Transfer the flower basket in step 4 to cleaning tank 2 and perform ultrasonic cleaning for 10 minutes.
[0108] 7. Transfer the flower basket to the sink and rinse it. Soak it in pure water 3 times.
[0109] 8. After completion, transfer the flower basket to the drying tank for hot nitrogen drying (hot nitrogen temperature is 60℃ and dried for 20 minutes).
[0110] 9. After drying, the silicon wafer is transferred to a silicon wafer box in a clean environment for glue coating.
[0111] Results: Figure 7 , BARC and photoresist layers remain on the surface of the silicon wafer. In addition, a large amount of reddish-brown smoke is produced when using nitric acid, which poses environmental pollution and health risks.
[0112] Comparative Example 2
[0113] The structure of the silicon wafer to be cleaned is as follows Figure 1 As shown, the 12-inch wafer was discarded after the company conducted photolithography process research. It was coated with a BARC layer (about 900 angstroms thick) and an ArF photoresist (about 1000 angstroms thick) and was exposed and developed. The cleaning and recycling method is as follows: Steps 1-9:
[0114] 1. Place 12 silicon wafers to be washed in a silicon wafer basket for later use.
[0115] 2. Prepare the acidic cleaning solution in cleaning tank 1: transfer 50L of hydrochloric acid (37%) and 10L of hydrogen peroxide (31%) to cleaning tank 1, heat and circulate and filter to 105°C.
[0116] 3. When the temperature of the acid cleaning solution in cleaning tank 1 reaches 105°C, carefully place the flower basket in 1 into the acid cleaning solution and soak for about 30 minutes.
[0117] 4. After soaking, transfer the flower basket to a hot water tank and rinse and soak for 10 minutes.
[0118] 5. Prepare alkaline cleaning solution in cleaning tank 2: transfer 5L ammonia water (30%), 10L hydrogen peroxide (31%) and 50L pure water to cleaning tank 2.
[0119] 6. Transfer the flower basket in step 4 to cleaning tank 2 and perform ultrasonic cleaning for 10 minutes.
[0120] 7. Transfer the flower basket to the sink and rinse it. Soak it in pure water 3 times.
[0121] 8. After completion, transfer the flower basket to the drying tank for hot nitrogen drying (hot nitrogen temperature is 60℃ and dried for 20 minutes).
[0122] 9. After drying, the silicon wafer is transferred to a silicon wafer box in a clean environment for glue coating.
[0123] Results: Figure 8 , there are BARC and photoresist layer residues on the surface of the silicon wafer.
[0124] Comparative Example 3
[0125] The structure of the silicon wafer to be cleaned is the same as that of the embodiment. Figure 1 As shown, the 12-inch wafer was discarded after the company conducted photolithography process research. It was coated with a BARC layer (about 900 angstroms thick) and an ArF photoresist (about 1000 angstroms thick) and was exposed and developed. The cleaning and recycling method is as follows: Steps 1-9:
[0126] 1. Place 12 silicon wafers to be washed in a silicon wafer basket for later use.
[0127] 2. Prepare the acid cleaning solution in cleaning tank 1: transfer 50L of dilute sulfuric acid (50%) and 10L of hydrogen peroxide (31%) to cleaning tank 1, heat and circulate and filter to 105°C.
[0128] 3. When the temperature of the acid cleaning solution in cleaning tank 1 reaches 105°C, carefully place the flower basket in 1 into the acid cleaning solution and soak for about 30 minutes.
[0129] 4. After soaking, transfer the flower basket to a hot water tank and rinse and soak for 10 minutes.
[0130] 5. Prepare alkaline cleaning solution in cleaning tank 2: transfer 5L ammonia water (30%), 10L hydrogen peroxide (31%) and 50L pure water to cleaning tank 2.
[0131] 6. Transfer the flower basket in step 4 to cleaning tank 2 and perform ultrasonic cleaning for 10 minutes.
[0132] 7. Transfer the flower basket to the sink and rinse it. Soak it in pure water 3 times.
[0133] 8. After completion, transfer the flower basket to the drying tank for hot nitrogen drying (hot nitrogen temperature is 60℃ and dried for 20 minutes).
[0134] 9. After drying, the silicon wafer is transferred to a silicon wafer box in a clean environment for glue coating.
[0135] Results: Fig. 9 , there are BARC and photoresist layer residues on the surface of the silicon wafer.
[0136] Comparative Example 4
[0137] The structure of the silicon wafer to be cleaned is as follows Figure 1 As shown, the 12-inch wafer was discarded after the company conducted photolithography process research. It was coated with a BARC layer (about 900 angstroms thick) and an ArF photoresist (about 1000 angstroms thick) and was exposed and developed. The cleaning and recycling method is as follows: Steps 1-9:
[0138] 1. Place 12 silicon wafers to be washed in a silicon wafer basket for later use;
[0139] 2. Prepare the acid cleaning solution in cleaning tank 1: transfer 50L sulfuric acid (98%) and 10L hydrogen peroxide (31%) to cleaning tank 1, heat and circulate and filter to 100°C.
[0140] 3. After the temperature of the acid cleaning solution in the cleaning tank 1 reaches 100°C, carefully place the flower basket in 1 into the heated acid cleaning solution and soak for about 30 minutes;
[0141] 4. After soaking, transfer the flower basket to a hot water tank and rinse and soak for 10 minutes.
[0142] 5. Prepare alkaline cleaning solution in cleaning tank 2: transfer 5L of ammonia water (30%), 10L of hydrogen peroxide (31%) and 50L of pure water to cleaning tank 2.
[0143] 6. Transfer the flower basket in step 4 to cleaning tank 2 and perform ultrasonic cleaning for 10 minutes.
[0144] 7. Transfer the flower basket to the sink and rinse it. Soak it in pure water 3 times.
[0145] 8. After completion, transfer the flower basket to the drying tank for hot nitrogen drying (hot nitrogen temperature is 60℃ and dried for 20 minutes).
[0146] 9. After drying, the silicon wafer is transferred to a silicon wafer box in a clean environment for glue coating.
[0147] Results: Fig.10 Although the surface of the silicon wafer is smooth, it is a black mirror, which means that the BARC layer has not been removed. The BARC layer cannot be removed under low temperature conditions.
[0148] In addition, after using the solution to clean 30 batches of 12 tablets per batch, the solution turned dark brown and had a strong odor and could no longer be used.
[0149] In summary, the method of the present invention can clean and remove the photoresist and / or BARC layer on the silicon wafer after exposure and development, and can be used to clean and recycle the silicon wafer after exposure. At the same time, the method of the present invention is simple, low-cost, and can be widely used.
[0150] In addition, it can be seen from the above results that the acid cleaning solution needs to maintain a relatively high temperature in order to dissolve and remove the photoresist and BARC layer on the silicon wafer. When the temperature is 100°C, the photoresist layer can be removed, but the BARC layer cannot be removed. As the temperature increases, the service life of the acid cleaning solution increases, but after the temperature rises to 135°C, the number of times the acid cleaning solution is used no longer increases. At the same time, as the temperature rises, the danger of the experimental operation will also increase. Therefore, when there is no BARC layer on the silicon wafer to be cleaned, the temperature of the acid cleaning solution can be 100°C or above. When there is a BARC layer and a photoresist layer on the silicon wafer to be cleaned, the acid cleaning solution needs to be soaked in the silicon wafer to be cleaned at 105°C or above, preferably 105°C to 135°C, and more preferably 105°C to 130°C. Therefore, by controlling the temperature of the acid cleaning solution, the service life of the acid cleaning solution can be increased and the experimental safety can be better guaranteed, further reducing the recovery cost of the silicon wafer before etching after exposure.
[0151] It should be noted that the exposed silicon wafer of the present invention is a silicon wafer that has been exposed and developed in a photolithography process and has not yet been etched. The photoresist on the silicon wafer undergoes a chemical reaction during the exposure process, and its properties are significantly different from those before exposure. The removal of the photoresist on the exposed silicon wafer of the present invention is also different from the removal of the photoresist after etching, and the etching process will have a further impact on the photoresist, such as the plasma environment may cause further crosslinking or degradation of the photoresist, and in the etching process, the photoresist as a mask needs to withstand physical and chemical attacks in the etching process, which will cause the loss or deformation of the photoresist. We use the method of the present invention to process the etched silicon wafer, and the degumming effect is not ideal. For example, ArF photoresist is a high-tech material designed for deep ultraviolet (DUV) lithography technology using a 193-nanometer argon fluorine laser light source. It is composed of resin, photoacid generator, solvent, additives, and other auxiliary materials. During the exposure process, the photoacid generator releases hydrogen ions, initiating a cross-linking reaction of the chemical chains in the resin; during the plasma etching process, the shape of the photoresist layer (mask) changes, and further cross-linking may occur.
[0152] It is understandable that those skilled in the art can, under the guidance of the above embodiments, combine various implementation methods in the above embodiments to obtain technical solutions of multiple implementation methods.
[0153] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for cleaning and recycling silicon wafers, characterized in that: The method comprises: S1. Place the silicon wafer to be cleaned in an acidic cleaning solution and soak it at 100°C or above for 10-60 minutes; S2. After soaking in the acid cleaning solution, washing with water to remove the residual acid cleaning solution on the surface of the silicon wafer; S3, placing the silicon wafer in an alkaline cleaning solution for 10-20 minutes; S4, after soaking in the alkaline cleaning solution, washing with water to remove the alkaline cleaning solution remaining on the surface of the silicon wafer, and drying for later use; The surface of the silicon wafer to be cleaned is coated with photoresist and subjected to exposure treatment; The acid cleaning solution comprises: sulfuric acid and hydrogen peroxide, wherein the content of sulfuric acid is higher than 80%; The alkaline cleaning solution comprises: ammonia water and hydrogen peroxide, wherein the content of the ammonia water is 5%-20%, and the content of the hydrogen peroxide is 5%-20%.
2. The method according to claim 1, characterized in that The acid cleaning solution consists of sulfuric acid, hydrogen peroxide and water, and the content of hydrogen peroxide is 5% to 15%.
3. The method according to claim 1, characterized in that The alkaline cleaning solution consists of ammonia water, hydrogen peroxide and water, the content of ammonia water is 5% to 15%, and the content of hydrogen peroxide is 10% to 15%.
4. The method according to claim 1, characterized in that The surface of the silicon wafer to be cleaned is also coated with a bottom anti-reflection coating, and in step S1, it is immersed at 105° C.-135° C. for 10 min-60 min.
5. The method according to claim 1, characterized in that The temperature of water in step S2 is 40°C-60°C.
6. The method according to claim 1, characterized in that In step S4, hot nitrogen is used for drying. The temperature of the hot nitrogen is 60° C. to 70° C., and the drying time is not less than 20 minutes.
7. The method according to claim 1, characterized in that The silicon wafer to be cleaned is a 12-inch wafer.
8. The method according to claim 1, characterized in that The photoresist is 193nm photoresist.
9. The method according to claim 1, characterized in that The thickness of the photoresist is 1000 angstroms to 2000 angstroms.
10. The method according to claims 1 to 9, characterized in that The acid cleaning solution in step S1 can be reused, but cannot be used when the acid cleaning solution turns dark brown.
Citation Information
Patent Citations
Method for removing SU-8 negative photoresist in cooperation with plasma etching and wet process
CN111045300A
Ozone-containing spray silicon wafer cleaning method
CN111151489A
Silicon wafer cleaning method for improving quality of metal and particles on surface of polished silicon wafer
CN116631848A
Reprocessing method for photoetching process
CN102543683A
Method for removing residual photoresist
CN103809395A