Copper alloy narrow-band continuous deep-cooling rolling device and process
By using liquid nitrogen protective shell and guide roller structure in the cryogenic rolling process, continuous cooling and tension increase of the narrow strip are achieved, which solves the problem of temperature rise of narrow plate or coiled materials during the rolling process and obtains high mechanical properties. and copper alloys with high electrical conductivity and reduced production costs.
Patent Information
- Application Number
- CN202410972323.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
When the existing cryogenic rolling process rolls narrow plates or coils with large dimensions in the rolling direction, the contact between the material and the air causes a temperature rise, which reduces the cryogenic treatment effect. In addition, the cost of equipment relocation and plant renewal is high, which limits the industrial promotion of the process. .
Design a copper alloy narrow strip continuous cryogenic rolling device, which uses a liquid nitrogen protective shell and guide roller structure to achieve continuous cooling and tension increase of the narrow strip during the rolling process by adjusting the rotation angle of the protective shell and the degree of liquid nitrogen immersion. Reduce heat exchange with the external environment.
Efficient continuous cryogenic rolling of narrow strips is achieved, and a copper alloy with ultra-fine grain/nano-twin structure with high mechanical properties and high electrical conductivity is obtained, which reduces the loss of cryogenic treatment effects and reduces production costs.
Smart Images

Figure CN118719801A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of copper alloy narrow strip rolling, and in particular relates to a copper alloy narrow strip continuous deep cold rolling device and process. Background Art
[0002] With the development of high-tech, the electrical and electronic field has put forward high requirements for high-strength and high-conductivity copper alloys with higher strength and better conductivity. Rare earth elements, which are known as "industrial vitamins", have a good modification effect on metal materials, especially copper alloys, including refining cast dendrites, promoting the precipitation of the second phase, purifying the matrix, etc. Therefore, rare earth copper alloys have great potential in achieving high-strength and high-conductivity comprehensive performance. In addition, studies have shown that twin boundaries have less scattering effect on electrons than general small / large angle grain boundaries, and the resistivity is even one order of magnitude lower than the latter. It is a feasible idea to introduce a large number of twin boundaries into copper alloys with low stacking fault energy to obtain better conductivity.
[0003] The large plastic deformation process is a preparation process for ultrafine grained / nano-twinned metal materials with ultra-high strength and good ductility. It can introduce a high proportion of ultrafine grains, nano-twinned crystals and high-density dislocations into the alloy, thereby preparing metal materials with excellent comprehensive performance. Large plastic deformation processes include equal-channel angular extrusion, high-pressure torsion, and the emerging deep cold rolling process in recent years. Unlike the equal-channel angular extrusion process that uses shear deformation to achieve grain refinement, the deep cold rolling process uses a deep cold environment to suppress the dynamic recovery of dislocation aggregation and annihilation during the deformation process of the alloy and the dynamic recrystallization of grains due to deformation heat to achieve the preparation of nanocrystalline materials. Compared with other large plastic deformation processes, the deep cold rolling process has unique advantages in achieving industrial production and reducing equipment transformation costs.
[0004] At present, the cryogenic rolling process usually combines cryogenic treatment of single-pass liquid nitrogen immersion before rolling with subsequent synchronous / asynchronous rolling. When preparing narrow plates or narrow strips with large rolling direction dimensions, the temperature rise caused by the contact of the material with the air during the rolling process will greatly reduce the effect of the cryogenic treatment. The usual solution is to place the entire rolling mill in a low-temperature enclosed space and reduce the working environment temperature to reduce the heat exchange between the material and the environment. However, equipment migration and plant renewal will bring high costs, which is not conducive to the industrial promotion and application of the cryogenic rolling process. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a copper alloy narrow strip continuous deep cold rolling device and process, so as to realize the continuous deep cold rolling of narrow plates or coiled copper alloy narrow strips with larger dimensions in the rolling direction, and prepare rare earth copper alloys with high mechanical properties and high electrical conductivity with ultrafine grains / nano twins, and the device and process also have lower cost.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A copper alloy narrow strip continuous deep cold rolling device comprises a first narrow strip coiler and a second narrow strip coiler, two ends of the narrow strip are respectively wound around the first narrow strip coiler and the second narrow strip coiler and can be driven to reciprocate between the two coilers; the first narrow strip coiler is located in a first protective shell with an opening, the second narrow strip coiler is located in a second protective shell with an opening, the first protective shell is opposite to the opening of the second protective shell, and the narrow strip passes through; an upper working roll and a lower working roll are arranged between the first protective shell and the second protective shell, the narrow strip is fully or partially immersed in a first liquid nitrogen in the first protective shell, and is fully or partially immersed in a second liquid nitrogen in the second protective shell, and passes through the roll gap between the upper working roll and the lower working roll outside the protective shell.
[0008] In one embodiment of the present invention, the top end of the first protective shell is connected to the first liquid nitrogen supply tank, and the bottom end is connected to the first liquid nitrogen recovery tank. The first liquid nitrogen in the first protective shell is provided by the first liquid nitrogen supply tank and is recovered by the first liquid nitrogen recovery tank. The top end of the second protective shell is connected to the liquid nitrogen supply tank, and the bottom end is connected to the liquid nitrogen recovery tank. The second liquid nitrogen in the second protective shell is provided by the second liquid nitrogen supply tank and is recovered by the second liquid nitrogen recovery tank.
[0009] In one embodiment of the present invention, a first guide roller is arranged at the opening position of the first protective shell, and a second guide roller is arranged at the opening position of the second protective shell. The first protective shell can rotate counterclockwise around the first guide roller by 20 to 30 degrees, and the second protective shell can rotate clockwise around the second guide roller by 20 to 30 degrees. The first guide roller and the second guide roller guide the narrow belt to remain horizontal after exiting the protective shell outlet.
[0010] In one embodiment of the present invention, the cross-section of the first protective shell and the second protective shell perpendicular to the roller axis is teardrop-shaped, the opening is located in the narrow part of the teardrop-shaped shape, and the winder is located in the wide part of the teardrop-shaped shape. By adjusting the rotation angle of the first protective shell around the first guide roller and the rotation angle of the second protective shell around the second guide roller, the immersion degree of the narrow belt of the winder in liquid nitrogen is adjusted, and the tension of the narrow belt is increased.
[0011] In one embodiment of the present invention, the first guide roller is partially immersed in the first liquid nitrogen in the first protective shell, the second guide roller is partially immersed in the second liquid nitrogen in the second protective shell, the narrow belt is fully or partially immersed in the first liquid nitrogen in the first protective shell, and fully or partially immersed in the second liquid nitrogen in the second protective shell, the first guide roller and the second guide roller guide the narrow belt to be immersed in the liquid nitrogen before exiting the protective shell outlet, and guide the narrow belt to remain horizontal after exiting the protective shell outlet.
[0012] In one embodiment of the present invention, the first narrow strip winder is installed in a first protective shell, and the first liquid nitrogen is contained in the first protective shell; the second narrow strip winder is installed in a second protective shell, and the second liquid nitrogen is contained in the second protective shell.
[0013] In one embodiment of the present invention, the first narrow strip winder and the second narrow strip winder are driven by independent motors respectively.
[0014] In one embodiment of the present invention, the upper working roll and the lower working roll adopt the same / different roll diameters and the same / different rotation speeds. When the rolling direction is changed alternately, the narrow strip coilers on both sides take turns as the raw material coiler and the product coiler.
[0015] In one embodiment of the present invention, the interval L1 between the first protective shell opening and the working roll is the same as the interval L2 between the second protective shell opening and the working roll, and L1 and L2 should be as small as possible without affecting the normal operation of the working roll. The smaller the value is, the shorter the contact time between the narrow belt and the external environment is, and the less heat is exchanged.
[0016] The present invention also provides a continuous deep cold rolling method using the copper alloy narrow strip continuous deep cold rolling device, comprising the following steps:
[0017] Step 1: Determine the distance between the protective shell and the working roll, install the first protective shell and the second protective shell, install one end of the narrow strip on the first narrow strip winder, pass the other end through the roll gap between the upper working roll and the lower working roll, and then set it on the second narrow strip winder;
[0018] Step 2: Start the first narrow strip winder and the second narrow strip winder to initially form tension on the narrow strip;
[0019] Step 3: rotate the first protective shell 20 to 30 degrees counterclockwise around the first guide roller, and rotate the second protective shell 20 to 30 degrees clockwise around the second guide roller, so as to further increase the tension of the narrow belt;
[0020] Step 4: Open the first liquid nitrogen supply tank and the second liquid nitrogen supply tank to add liquid nitrogen to the first protective shell and the second protective shell until they are full, and maintain continuous supply;
[0021] Step 5: Open the upper working roll and the lower working roll, set the single-pass roll gap and start rolling until the effective length of the narrow strip on the first narrow strip coiler has been rolled;
[0022] Step 6: Pause the rolling mill and change the rolling direction.
[0023] Step 7: Open the upper working roll and the lower working roll, set the single-pass roll gap and start rolling until the effective length of the narrow strip on the second narrow strip coiler has been rolled;
[0024] Step 8: Pause the rolling mill and change the rolling direction.
[0025] Step 9: Repeat steps 5 to 8, and continue production until the thickness of the narrow strip reaches the target total rolling deformation, and the rolling is completed.
[0026] Step 10: Open the first liquid nitrogen recovery tank and the second liquid nitrogen recovery tank to recover the remaining liquid nitrogen;
[0027] Step 11: Rotate the first protective shell 20 to 30 degrees clockwise around the first guide roller, and rotate the second protective shell 20 to 30 degrees counterclockwise around the second guide roller, remove the tension on the narrow belt, and take the narrow belt off from the narrow belt winder on one side.
[0028] In one embodiment of the present invention, the narrow strip is a strip having a width of 50 to 200 mm and can be slightly bent or completely bent into a coil, and the copper alloy component is a high-strength and high-conductivity copper alloy such as a Cu-Ag alloy.
[0029] In one embodiment of the present invention, the copper alloy narrow strip is subjected to the continuous deep cold rolling method, and the total rolling reduction rate reaches more than 90%. The obtained product has a strength greater than or equal to 600MPa, a Vickers hardness greater than or equal to 200HV, and a conductivity greater than or equal to 60%IACS, and has high mechanical properties and high conductivity.
[0030] Compared with the prior art, the beneficial effects of the present invention are: it can greatly reduce the unnecessary loss of cryogenic treatment effect in the process of cryogenic rolling in the links of material transportation and transmission, and obtain more rigorous and accurate experimental conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the structure of the device of the present invention.
[0032] Figure 2 It is a schematic diagram of the structure of the device of the present invention (adjusting the angle of the protective shell).
[0033] In the figure:
[0034] 1—first guide roller; 2—first liquid nitrogen recovery tank; 3—first liquid nitrogen supply tank; 4—first narrow strip coiler; 5—narrow strip; 6—first protective shell; 7—upper working roller; 8—second protective shell; 9—second narrow strip coiler; 10—second liquid nitrogen supply tank; 11—second liquid nitrogen recovery tank; 12—second guide roller; 13—lower working roller; 14—first liquid nitrogen; 15—second liquid nitrogen. DETAILED DESCRIPTION
[0035] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.
[0036] like Figure 1 and Figure 2 As shown, a copper alloy narrow strip continuous deep cold rolling device of the present invention is composed of three parts: a narrow strip protection device that can realize continuous cooling, a liquid nitrogen supply / recovery device, and a structure that can realize continuous forward and reverse different speed / asynchronous rolling. The first part of the narrow strip protection device mainly includes a first guide roller 1, a first protective shell 6, a second protective shell 8, and a second guide roller 12. The first protective shell 6 contains a first liquid nitrogen 14, and the second protective shell 8 contains a second liquid nitrogen 15. The two protective shells have openings, and the openings are opposite. The two guide rollers are respectively arranged at the openings of the two protective shells, and the protective shells can rotate around the guide rollers at a certain angle (20 to 30 degrees). The second part of the liquid nitrogen supply / recovery device mainly includes a first liquid nitrogen recovery tank 2, a first liquid nitrogen supply tank 3, a second liquid nitrogen supply tank 10, and a second liquid nitrogen recovery tank 11. The liquid nitrogen supply tank continuously provides liquid nitrogen to the inner cavity of the two protective shells, and the excess liquid nitrogen can be recovered by the liquid nitrogen recovery tank after the processing is completed. The third part of the continuous forward and reverse speed / asynchronous rolling structure mainly includes the first narrow strip coiler 4, the second narrow strip coiler 9, the upper working roll 7 and the lower working roll 13. The first narrow strip coiler 4 is arranged in the first protective shell 6, and the second narrow strip coiler 9 is arranged in the second protective shell 8. The upper working roll 7 and the lower working roll 13 are opposite to each other, and a roll gap is formed between them. The upper working roll 7 and the lower working roll 13 are between the openings of the two protective shells, so that the narrow strip 5 can pass through the roll gap. One end of the narrow strip 5 to be rolled is installed on the first narrow strip coiler 4 on one side, and the other end is arranged on the second narrow strip coiler 9 on the other side after passing through the roll gap between the upper working roll 7 and the lower working roll 13, and tension is formed. The rotation of the protective shell around the guide roller makes the narrow strip 5 in the first protective shell 6 and the second protective shell 8 completely or partially immersed in liquid nitrogen, and the tension in the narrow strip 5 is increased. The narrow strip 5 should be completely immersed in liquid nitrogen before passing through the outlet of the first protective shell 6 and the second protective shell 8.
[0037] The main principle of the present invention is to use a cylindrical container to simultaneously hold liquid nitrogen and a rolled narrow strip, thereby achieving continuous cooling of the material before entering the rolling roller and after leaving the rolling roller, shortening the time and scale of the material's contact with the external environment during transportation and transmission, ensuring a long-term stable low-temperature deformation environment, inhibiting the dynamic recovery of dislocations, increasing the density of crystal defects such as dislocations and grain boundaries in the alloy, and improving the performance of the copper alloy.
[0038] In an embodiment of the present invention, the cross-section of the first protective shell 6 and the second protective shell 8 perpendicular to the roller axis direction is teardrop-shaped, the opening of the protective shell is located at the narrow part of the teardrop shape, the first narrow strip winder 4 and the second narrow strip winder 9 are respectively located at the wide part of the teardrop shape, and by adjusting the rotation angle of the first protective shell 6 around the first guide roller 1 and the rotation angle of the second protective shell 8 around the second guide roller 12, the immersion degree of the narrow strip 5 on the winder in the corresponding liquid nitrogen can be adjusted, and the tension on the narrow strip 5 can be increased.
[0039] In an embodiment of the present invention, the first narrowband winder 4 and the second narrowband winder 9 are respectively installed on the first protective shell 6 and the second protective shell 8, and are driven by independent motors. The diameters R1 and R3 and the internal cavity sizes R2 and R4 of the shells can be set according to the actual narrowband size or other requirements.
[0040] In the embodiment of the present invention, the shell walls of the first protective shell 6 and the second protective shell 8 may be filled with vacuum or thermal insulation cotton to improve the thermal insulation effect and reduce the loss of liquid nitrogen. Thermal insulation measures may also be taken at each gap.
[0041] In the embodiment of the present invention, a first guide roller 1 is provided between the first narrow strip coiler 4 and the upper working roller 7, and a second guide roller 12 is provided between the second narrow strip coiler 9 and the lower working roller 13. The first guide roller 1 is mounted on the first protective shell 6 and is arranged near the protective shell outlet. The second guide roller 12 is mounted on the second protective shell 8 and is arranged near the protective shell outlet. The function of the two guide rollers is to ensure that the narrow strip 5 is parallel to the plane where the roll gap is when entering and leaving the roll gap of the working rollers as much as possible, and is immersed in liquid nitrogen before passing through the outlet.
[0042] In the embodiment of the present invention, the first liquid nitrogen recovery tank 2, the first liquid nitrogen supply tank 3, the second liquid nitrogen supply tank 10 and the second liquid nitrogen recovery tank 11 are provided with switches for easy control.
[0043] In the embodiment of the present invention, the upper working roll 7 and the lower working roll 13 can adopt the same / different roll diameters and the same / different rotation speeds. When the rolling direction is changed alternately, the narrow strip coilers on both sides take turns as the raw material coiler and the product coiler.
[0044] In an embodiment of the present invention, the distances L1 and L2 between the narrow band protection structures on both sides and the working rolls are the same, and the value should be as small as possible without affecting the normal operation of the working rolls. The smaller the value, the shorter the contact time between the narrow band and the external environment, and the less heat is exchanged.
[0045] According to the copper alloy narrow strip continuous deep cold rolling device of the present invention, the corresponding continuous deep cold rolling method comprises the following steps:
[0046] Step 1: Determine reasonable distances L1 and L2, place the first protective shell 6 and the second protective shell 8, install one end of the narrow strip 5 on the first narrow strip winder 4, and pass the other end through the gap between the upper working roll 7 and the lower working roll 13, and then place it on the second narrow strip winder 10;
[0047] Step 2: Start the first narrow strip winder 4 and the second narrow strip winder 10 to initially form tension on the narrow strip 5;
[0048] Step 3: Make the first protective shell 6 rotate 20 to 30 degrees counterclockwise around the first guide roller 1, and the second protective shell 8 rotate 20 to 30 degrees clockwise around the second guide roller 12, so as to further increase the tension of the narrow belt 5. Figure 2 As shown;
[0049] Step 4: Open the first liquid nitrogen supply tank 3 and the second liquid nitrogen supply tank 10 to add liquid nitrogen to the first protective shell 6 and the second protective shell 8 until they are full, and maintain continuous supply;
[0050] Step 5: Open the upper working roll 7 and the lower working roll 13, set a single-pass roll gap and start rolling until the effective length of the narrow strip 5 on the first narrow strip coiler 4 has been rolled;
[0051] Step 6: Pause the rolling mill and change the rolling direction.
[0052] Step 7: Open the upper working roll 7 and the lower working roll 13, set a single-pass roll gap and start rolling until the effective length of the narrow strip 5 on the second narrow strip coiler 10 has been rolled;
[0053] Step 8: Pause the rolling mill and change the rolling direction.
[0054] Step 9: Repeat steps 5 to 8, and continue production until the thickness of the narrow strip reaches the target total rolling deformation, and the rolling is completed.
[0055] Step 10: Open the first liquid nitrogen recovery tank and the second liquid nitrogen recovery tank to recover the remaining liquid nitrogen;
[0056] Step 11: Rotate the first protective shell 6 20 to 30 degrees clockwise around the first guide roller 1, and rotate the second protective shell 8 20 to 30 degrees counterclockwise around the second guide roller 12, remove the tension on the narrow belt 5, and take down the narrow belt 5 from the narrow belt winder on one side.
[0057] Taking the continuous deep cold rolling of Cu-5Ag-0.55Ce (wt.%) copper alloy narrow strip as an example, it includes the following steps:
[0058] Step 1: Determine a reasonable distance L1=L2=5 mm, place the first protective shell 6 and the second protective shell 8, install one end of the narrow strip 5 on the first narrow strip winder 4, and pass the other end through the gap between the upper working roll 7 and the lower working roll 13, and then place it on the second narrow strip winder 10;
[0059] Step 2: Start the first narrow strip winder 4 and the second narrow strip winder 10 to initially form tension on the narrow strip 5, the tension being 30 MPa;
[0060] Step 3: rotate the first protective shell 6 25 degrees counterclockwise around the first guide roller 1, and rotate the second protective shell 8 25 degrees clockwise around the second guide roller 12, further increasing the tension of the narrow belt 5 to about 40 MPa;
[0061] Step 4: Open the first liquid nitrogen supply tank 3 and the second liquid nitrogen supply tank 10 to add liquid nitrogen to the first protective shell 6 and the second protective shell 8 until they are full, and maintain continuous supply;
[0062] Step 5: Open the upper working roll 7 and the lower working roll 13, set the single-pass deformation amount to 5%, and start rolling until the effective length of the narrow strip 5 on the first narrow strip coiler 4 has been rolled;
[0063] Step 6: Pause the rolling mill and change the rolling direction.
[0064] Step 7: Open the upper working roll 7 and the lower working roll 13, set the single-pass deformation amount to 5%, and start rolling until the effective length of the narrow strip 5 on the second narrow strip coiler 10 has been rolled;
[0065] Step 8: Pause the rolling mill and change the rolling direction.
[0066] Step 9: Repeat steps 5 to 8, and continue production until the total rolling deformation of the narrow strip is 90%, and the rolling is completed;
[0067] Step 10: Open the first liquid nitrogen recovery tank and the second liquid nitrogen recovery tank to recover the remaining liquid nitrogen;
[0068] Step 11: Rotate the first protective shell 6 25 degrees clockwise around the first guide roller 1, and rotate the second protective shell 8 25 degrees counterclockwise around the second guide roller 12, remove the tension on the narrow belt 5, and take down the narrow belt 5 from the narrow belt winder on one side.
[0069] The performance statistics of the alloy finally obtained are shown in Table 1
[0070] Table 1 Cu-Ag-Ce alloy performance statistics
[0071] performance Measured value 1 Measured value 2 Measured value 3 Measured value 4 Measured value 5 average value Standard Deviation Vickers hardness 215.2 221.4 222.7 220.2 224.0 220.70 3.39 Electrical conductivity 69.4 66.8 68.1 65.8 67.1 67.44 1.36 Yield Strength 623 609 622 — — 618.0 7.8 Ultimate tensile strength 639 636 658 — — 644.3 11.9
Claims
1. A copper alloy narrow strip continuous deep cold rolling device, characterized in that: The invention comprises a first narrow-belt reel (4) and a second narrow-belt reel (10), wherein a narrow-belt (5) is wound on the first narrow-belt reel (4) and the second narrow-belt reel (10) and can be driven to reciprocate between the two reels; the first narrow-belt reel (4) is located in a first protective shell (6) with an opening, and the second narrow-belt reel (10) is located in a second protective shell (8) with an opening, and the openings of the first protective shell (6) and the second protective shell (8) are opposite to each other, so that the narrow-belt (5) can pass through; An upper working roll (7) and a lower working roll (13) are arranged between the first protective shell (6) and the second protective shell (8); the narrow strip (5) is fully or partially immersed in a first liquid nitrogen (14) in the first protective shell (6), fully or partially immersed in a second liquid nitrogen (15) in the second protective shell (8), and passes through a roll gap between the upper working roll (7) and the lower working roll (13) outside the protective shell.
2. The copper alloy narrow strip continuous deep cold rolling device according to claim 1, characterized in that: The top end of the first protective shell (6) is connected to the first liquid nitrogen supply tank (3), and the bottom end is connected to the first liquid nitrogen recovery tank (2); the first liquid nitrogen (14) in the first protective shell is provided by the first liquid nitrogen supply tank (3) and is recovered by the first liquid nitrogen recovery tank (2); The top end of the second protective shell (8) is connected to the second liquid nitrogen supply tank (10), and the bottom end is connected to the second liquid nitrogen recovery tank (11); the second liquid nitrogen (15) in the second protective shell is provided by the second liquid nitrogen supply tank (10) and is recovered by the second liquid nitrogen recovery tank (11).
3. The copper alloy narrow strip continuous deep cold rolling device according to claim 1, characterized in that: A first guide roller (1) is arranged at the opening position of the first protective shell (6), and a second guide roller (12) is arranged at the opening position of the second protective shell (8). The first protective shell (6) can rotate 20 to 30 degrees counterclockwise around the first guide roller (1), and the second protective shell (8) can rotate 20 to 30 degrees clockwise around the second guide roller (12). The first guide roller (1) and the second guide roller (12) guide the narrow belt (5) to remain horizontal after exiting the protective shell outlet.
4. The copper alloy narrow strip continuous deep cold rolling device according to claim 3, characterized in that: The cross-sections of the first protective shell (6) and the second protective shell (8) perpendicular to the roller axis are teardrop-shaped, the opening is located at the narrow part of the teardrop-shaped shape, and the winder is located at the wide part of the teardrop-shaped shape. By adjusting the rotation angle of the first protective shell (6) around the first guide roller (1) and the rotation angle of the second protective shell (8) around the second guide roller (12), the immersion degree of the narrow strip (5) of the winder in the liquid nitrogen is adjusted, and the tension of the narrow strip (5) is increased.
5. The copper alloy narrow strip continuous deep cold rolling device according to claim 1, characterized in that: The first guide roller (1) is partially immersed in the first liquid nitrogen (14) in the first protective shell (6), and the second guide roller (12) is partially immersed in the second liquid nitrogen (15) in the second protective shell (8). The narrow belt (5) is fully or partially immersed in the first liquid nitrogen (14) in the first protective shell (6), and fully or partially immersed in the second liquid nitrogen (15) in the second protective shell (8). The first guide roller (1) and the second guide roller (12) guide the narrow belt (5) to be immersed in the liquid nitrogen before exiting the protective shell outlet, and guide the narrow belt (5) to remain horizontal after exiting the protective shell outlet.
6. The copper alloy narrow strip continuous deep cold rolling device according to claim 1, characterized in that: The first narrow strip coiler (4) and the second narrow strip coiler (10) are driven by independent motors respectively; the upper working roll (7) and the lower working roll (13) have the same / different roll diameters and the same / different rotation speeds. When the rolling direction is changed alternately, the narrow strip coilers on both sides take turns to serve as a raw material coiler and a product coiler.
7. The copper alloy narrow strip continuous deep cold rolling device according to claim 1, characterized in that: The interval L1 between the opening of the first protective shell (6) and the working roller is the same as the interval L2 between the opening of the second protective shell (8) and the working roller, and L1 and L2 should be as small as possible without affecting the normal operation of the working roller. The smaller the value, the shorter the contact time between the narrow belt (5) and the external environment, and the less heat is exchanged.
8. A continuous deep cold rolling method using the copper alloy narrow strip continuous deep cold rolling device according to any one of claims 1 to 7, characterized in that: The steps include: The first step is to determine the distance between the protective shell and the working roll, install the first protective shell (6) and the second protective shell (8), install one end of the narrow strip (5) on the first narrow strip coiler (4), pass the other end through the roll gap between the upper working roll (7) and the lower working roll (13), and then set it on the second narrow strip coiler (10); Step 2: starting the first narrow strip winder (4) and the second narrow strip winder (10) to initially form tension on the narrow strip (5); Step 3: rotating the first protective shell (6) counterclockwise by 20 to 30 degrees around the first guide roller (1), and rotating the second protective shell (8) clockwise by 20 to 30 degrees around the second guide roller (12), so as to further increase the tension of the narrow belt (5); Step 4: Open the first liquid nitrogen supply tank (3) and the second liquid nitrogen supply tank (10) to add liquid nitrogen to the first protective shell (6) and the second protective shell (8) until they are full, and maintain continuous supply; Step 5: Open the upper working roll (7) and the lower working roll (13), set a single-pass roll gap and start rolling until the effective length of the narrow strip (5) on the first narrow strip coiler (4) has been rolled; Step 6: Pause the rolling mill and change the rolling direction; Step 7: Open the upper working roll (7) and the lower working roll (13), set a single-pass roll gap and start rolling until the effective length of the narrow strip (5) on the second narrow strip coiler (10) has been rolled; Step 8: Pause the rolling mill and change the rolling direction; Step 9: Repeat steps 5 to 8, and continue production until the thickness of the narrow strip reaches the target total rolling deformation, and the rolling is completed. Step 10: Open the first liquid nitrogen recovery tank (2) and the second liquid nitrogen recovery tank (11) to recover the remaining liquid nitrogen; Step 11: Rotate the first protective shell (6) around the first guide roller (1) by 20 to 30 degrees clockwise, and rotate the second protective shell (8) around the second guide roller (12) by 20 to 30 degrees counterclockwise, remove the tension on the narrow belt (5), and remove the narrow belt (5) from the narrow belt winder on one side.
9. The continuous deep cold rolling method according to claim 8, characterized in that: The copper alloy component is a Cu-Ag alloy, and the narrow strip (5) is a strip material with a width of 50 to 200 mm and can be slightly bent or completely bent into a coil.
10. The continuous deep cold rolling method according to claim 8, characterized in that: When the copper alloy narrow strip is Cu-5Ag alloy, after the continuous deep cold rolling method, the total rolling reduction rate reaches more than 90%, the product strength is greater than or equal to 600MPa, the Vickers hardness is greater than or equal to 200HV, and the conductivity is greater than or equal to 60%IACS.
Citation Information
Patent Citations
Continuous and reversible copious cooling rolling process and equipment for preparing high-performance aluminum alloy strip for car
CN108296286A
Strong pulse current assisted deep-cooling reducing asynchronous rolling device and method for preparing ultrafine grain metal strip
CN109092897A
High-intensity pulse current assisted deep cold rolling device and method for preparing ultra-fine grain metal strips
CN109108070A
Strong impulse current auxiliary copious cooling different speed asynchronous rolling device and method for preparing ultra-fine grain metal strip
CN109174968A
Compound rolling preparation method of gradient structure strip
CN109201738A