Preparation method of low-cost laminated hard alloy spherical teeth for mining

By adopting a stacked design of high hardness layer and high toughness layer in the cemented carbide ball teeth, combined with recycled WC powder and multi-layer transition layer, the performance contradiction of traditional cemented carbide materials in high wear resistance and high impact environments is solved. And the problem of high cost has significantly improved the overall performance and service life of the material.

CN118720144APending Publication Date: 2024-10-01HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410989621.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional carbide ball tooth materials are difficult to balance hardness and fracture toughness at the same time, and the production cost is high. They are prone to cracking in high wear resistance and high impact environments. The shortage of raw materials such as tungsten and cobalt has led to price increases.

Method used

It adopts the design of laminated carbide ball teeth, through the combination of high hardness layer and high toughness layer. The high hardness layer is composed of recycled fine WC powder, Co powder and Y2O3. The high toughness layer is composed of multiple transition layers. The bonding surface and ball The direction of the tooth spherical surface is consistent, and the thickness of each layer gradually increases. It is prepared through wet grinding, calcination and sintering processes to ensure that the material transmits load evenly during application and improves the impact buffering effect.

Benefits of technology

It achieves a balance between hardness and fracture toughness, reduces production costs, improves the wear and impact resistance of the material, extends the service life and reduces maintenance costs, and avoids the performance mutation and stress concentration problems of traditional gradient cemented carbide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 8FFIQVTAP8QBK2WOXPQAHWYGICHXXFQD5KEHUVFL
    Figure 8FFIQVTAP8QBK2WOXPQAHWYGICHXXFQD5KEHUVFL
  • Figure QZ9I8FQAODZ2UMMD6KTVECZGCWI78BVPYZAGMDWY
    Figure QZ9I8FQAODZ2UMMD6KTVECZGCWI78BVPYZAGMDWY
  • Figure RNOFRWKW9TLAQDEEQDMX1JI5Q6QY2HFMJAIMQZQP
    Figure RNOFRWKW9TLAQDEEQDMX1JI5Q6QY2HFMJAIMQZQP
Patent Text Reader

Abstract

The invention discloses a preparation method of a low-cost laminated hard alloy spherical tooth for mining. The preparation method comprises the following steps: step 1, preparing a high-hardness layer material; 2, preparing a high-toughness layer material; and 3, forming and sintering the laminated hard alloy ball teeth. The problem that hardness and fracture toughness of a traditional homogeneous hard alloy are difficult to consider at the same time is solved in a mode of combining a high-hardness layer material and a high-toughness layer material; the design of combining multiple layers and special structures improves the contact area and bonding strength between layers, ensures that the alloy uniformly transmits load in the application process, and improves the impact buffering effect; the regenerated WC powder is used as a hard phase material, and a strengthening phase is doped in a solid-liquid manner, so that the distribution uniformity of the strengthening phase is ensured, the comprehensive performance of the regenerated WC powder is improved, and meanwhile, the preparation cost is greatly reduced; the prepared laminated hard alloy material and the spherical tooth have high wear resistance and high impact resistance, and the service life and the efficiency of the hard alloy under complex and harsh working conditions are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of cemented carbide material preparation, and specifically relates to a method for preparing a stacked cemented carbide button, and more specifically relates to a method for preparing a low-cost stacked cemented carbide button for mining. Background Art

[0002] Cemented carbide is widely used in wear-resistant parts, mining tools and other fields due to its many excellent properties such as high hardness, high strength and high wear resistance. At present, conventional cemented carbide ball gear materials are composed of homogeneous microstructures. This homogeneous microstructure makes it difficult to take into account both hardness and fracture toughness at the same time, so it is difficult to meet the high wear resistance and high impact performance requirements in high-hard rock drilling environments, which limits its application to a certain extent. Gradient cemented carbide can effectively solve the contradiction between hardness and toughness. However, traditional gradient cemented carbide has problems such as sudden change in the performance of the gradient layer, decarburization phase and stress concentration in the inner layer, so it is easy to crack during application. Nowadays, the demand for cemented carbide ball gears continues to increase, while tungsten and cobalt, the raw materials of cemented carbide ball gears, are non-renewable resources. Their reserves are decreasing year by year, and the problem of resource shortage is becoming increasingly serious, resulting in a continuous increase in the price of cemented carbide ball gears. Therefore, it is of great practical significance and economic value to develop cemented carbide ball gear materials with high hardness, high toughness and low cost, and to realize industrial production. Summary of the invention

[0003] In view of the deficiencies raised in the above-mentioned background technology, the present invention studies and designs a method for preparing low-cost stacked cemented carbide ball teeth for mining, aiming to solve many problems such as it is difficult to take into account both the hardness and fracture toughness of conventional cemented carbide ball teeth, the easy cracking of conventional gradient cemented carbide during application and the high production cost of cemented carbide ball teeth.

[0004] The technical solution of the present invention: A low-cost laminated cemented carbide ball tooth for mining, consisting of at least two major parts, namely a high-hardness layer and a high-toughness layer, wherein the thickness ratio of the high-hardness layer to the high-toughness layer is 1:2-4, the high-hardness layer consists of a matrix phase and a hard phase, and the high-toughness layer consists of at least two transition layers, the bonding surfaces between the layers are consistent with the spherical surface direction of the ball tooth, and the curvature of the bonding surface of each layer decreases from top to bottom and is embedded in the bonding surface of the previous layer, and the thickness of each layer gradually increases, thereby ensuring that the ball tooth transmits load evenly during application, improving the buffering effect during impact, and thus avoiding performance mutations.

[0005] A method for preparing a low-cost laminated cemented carbide button for mining, comprising the following steps: Step 1: Preparation of high hardness layer material (1) The hard phase is composed of recycled fine WC powder, Co powder and Y2O3, wherein the mass fraction of Co is 5%-8%, the mass fraction of Y2O3 is 0%-1%, and the balance is recycled fine WC powder. The hard phase is prepared by wet grinding and spray drying the recycled fine WC powder, Co powder and fully dissolved Y(NO3)3 solution, and then calcining the mixed powder in a tube furnace. After the mixed powder is cooled to room temperature, it is graded and sieved to obtain the hard phase; (2) The matrix phase is composed of coarse WC powder and Co powder, wherein the mass fraction of Co is 8%-10% and the remainder is coarse WC powder. The matrix phase is prepared by wet grinding the coarse WC powder and Co powder and then sieving to obtain the matrix phase; (3) The hard phase and the matrix phase are uniformly mixed according to the corresponding configuration ratio, so that the hard phase is evenly distributed in the matrix phase, thereby obtaining a high hardness layer material; Step 2: Preparation of high-toughness layer material (1) The high-toughness layer material is composed of coarse WC powder and Co powder, wherein the mass fraction of Co is 10%-14% and the remainder is coarse WC. The coarse WC powder and Co powder are wet-grinded and then dried and sieved to obtain the high-toughness layer material; (2) The high-toughness layer material is composed of at least two layers of transition layer materials, in which the thickness of each transition layer gradually increases from top to bottom, and the Co content of each layer also increases from top to bottom; Step 3: Forming and sintering of laminated carbide ball gears The prepared high-hardness layer material and high-toughness material are powdered layer by layer and then pressed to obtain a pressed green body, which is then sintered in a low-pressure sintering furnace to obtain a stacked cemented carbide ball gear material.

[0006] Preferably, in the raw materials for preparing the hard phase in step 1, the particle size of the recycled WC powder is 1-2 μm, the particle size of the Co powder is 1-2 μm, the purity of Y(NO3)3 is 99.9%, and Y2O3 is obtained by thermal decomposition of Y(NO3)3.

[0007] Preferably, when preparing the hard phase in step 1, the calcination temperature is 850°C-1100°C, the calcination time is 1-3h, and after calcination, it is cooled to room temperature, wherein the heating rate is 10°C / min, and the cooling rate is 10°C / min.

[0008] Preferably, in the raw materials for preparing the matrix phase in step 1, the particle size of the coarse WC powder is 4-8 μm, and the particle size of the Co powder is 1-2 μm.

[0009] Preferably, in the step 1, the hard phase and the matrix phase are mixed by heating and mechanical stirring, the heating temperature is 50-60° C., and the mixing time is 2-6 hours.

[0010] Preferably, in step 1, the mass percentage of the hard phase added is 50%-80%, the mass percentage of the matrix phase added is 20%-50%, and the amount of the molding agent added is 2%-4% of the total weight of the hard phase and the matrix phase.

[0011] Preferably, the thickness of the high hardness layer material in step 1 is ≥4 mm.

[0012] Preferably, in the step 2, the particle size of the coarse WC powder in the high-toughness layer material is 4-8 μm, and the particle size of the Co powder is 1-2 μm.

[0013] Preferably, in the step 2, the thickness of the high-toughness layer material is ≥8 mm, and the ratio of the thickness of the transition layer is 1:1.5.

[0014] Preferably, in step three, the sintering temperature is 1410-1460° C., the sintering time is 1-2 h, and the sintering pressure is ≥5 MPa.

[0015] Beneficial effects of the present invention: (1) The present invention solves the problem that it is difficult to simultaneously take into account the hardness and fracture toughness of traditional homogeneous cemented carbide by combining a high-hardness layer material with a high-toughness layer material; (2) The present invention helps to increase the contact area and bonding strength between layers through a design combining multiple layers and special structures, which can ensure that the alloy transfers loads evenly during application, improve the impact buffering effect, and solve the problems of gradient layer performance mutation and stress concentration in traditional gradient cemented carbide; (3) The present invention uses recycled WC powder as the hard phase material and dopes the strengthening phase with solid and liquid, which not only ensures the uniformity of the strengthening phase distribution, but also improves the comprehensive performance of the recycled WC powder, and also greatly reduces the preparation cost; (4) The laminated cemented carbide material and ball gear prepared by the present invention have both high wear resistance and high impact resistance, which solves the problems of fast wear, poor durability and high cost of ordinary ball gear materials in the prior art, and significantly improves the service life and efficiency of cemented carbide under complex and harsh working conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the structure of the stacked cemented carbide ball gear in the present invention; Among them: A, high hardness layer, B, high toughness layer, 1, hard phase, 2, matrix phase; Figure 2 This is a low-magnification microstructure diagram of the laminated cemented carbide high-hardness layer of Example 1 of the present invention; Figure 3 This is a high-magnification microstructure diagram of the laminated cemented carbide high-hardness layer of Example 1 of the present invention; Figure 4This is a diagram of the interface organization of the stacked cemented carbide high-hardness layer and high-toughness layer of Example 1 of the present invention. DETAILED DESCRIPTION

[0017] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0018] Example 1 like Figure 1 As shown, the stacked carbide ball tooth in this embodiment consists of two major parts, namely a high hardness layer A and a high toughness layer B, wherein the high hardness layer A consists of a hard phase 1 and a matrix phase 2, and the high toughness layer B consists of two transition layers. In order to ensure the bonding strength of the bonding surface and uniformly transfer the load, the bonding surface between the layers is consistent with the spherical surface direction of the ball tooth, and the curvature of each bonding surface decreases from top to bottom and is embedded in the bonding surface of the previous layer, and the thickness of each transition layer gradually increases.

[0019] The specific preparation steps of the stacked carbide button gear in this embodiment are: Step 1: Preparation of high hardness layer material (1) The hard phase is composed of recycled fine WC powder with a particle size of 1.5 μm, 1 μm Co powder and Y2O3, wherein the mass fraction of recycled fine WC powder is 93.5%; the mass fraction of Co powder is 6%; and the mass fraction of Y2O3 is 0.5%. When preparing the hard phase, the recycled fine WC powder, Co powder and fully dissolved Y(NO3)3 solution are wet-milled with alcohol as the wet-milling medium for 32 h, followed by spray drying. The dried mixed powder is then loaded into a tubular furnace for high-temperature calcination at a temperature of 1050°C for 2.5 h. Finally, the calcined and cooled mixed powder is sieved to obtain the hard phase. (2) The matrix phase is composed of coarse WC powder with a particle size of 7 μm and Co powder with a particle size of 1 μm, wherein the mass fraction of the coarse WC powder is 90% and the mass fraction of the Co powder is 10%. When preparing the matrix phase, the coarse WC powder and the Co powder are wet-milled, the wet-milling medium is alcohol, and the wet-milling time is 20 h. After the wet-milling, the mixed slurry is sieved to obtain the matrix phase; (3) 70% by weight of the hard phase and 30% by weight of the matrix phase were fully mixed at 55°C for 3 hours, paraffin was added as a molding agent during the mixing, and the amount of paraffin added was 3% of the total weight of the hard phase and the matrix phase. After being fully mixed, the mixture was dried at 85°C in a vacuum drying oven for 2.5 hours, and then sieved and granulated to finally obtain a high hardness layer material; (4) In order to ensure that the high hardness layer has sufficient wear resistance and strength, the thickness of the high hardness layer is set to 5 mm; Step 2: Preparation of high-toughness layer material (1) The high-toughness layer material is a two-layer transition layer material, which is composed of coarse WC powder with a particle size of 7 μm and Co powder with a particle size of 1 μm. When preparing the high-toughness layer material, the coarse WC powder and Co powder are wet-milled. The wet-milling medium is alcohol. The wet-milling time is 22 h. After the wet-milling, they are dried at 85 °C in a vacuum drying oven for 2.5 h, and then sieved and granulated to obtain the high-toughness layer material; (2) To ensure that the high-toughness layer has sufficient bending strength, fracture toughness, uniform stress distribution and can evenly transfer load, the mass fractions of coarse WC powder in each transition layer from top to bottom are 88% and 86% respectively; the mass fractions of Co powder are 12% and 14% respectively, and the thickness of the transition layer is prepared at a ratio of 1:1.5, where the thickness of the first transition layer is set to 4 mm; Step 3: Forming and sintering of laminated carbide ball gear materials The prepared high-hardness layer material and high-toughness material are powdered layer by layer and then pressed to obtain a pressed green body, which is then sintered at 1410°C in a low-pressure sintering furnace for 1.5 hours at a sintering pressure of 6 MPa. After sintering, a stacked cemented carbide ball gear material can be obtained. The properties of the stacked cemented carbide material prepared by the above process are shown in Table 1.

[0020] Example 2 like Figure 1 As shown, the stacked cemented carbide material in this embodiment consists of two major parts, namely, a high-hardness layer A and a high-toughness layer B, wherein the high-hardness layer A consists of a hard phase 1 and a matrix phase 2, and the high-toughness layer B consists of two transition layers. In order to ensure the bonding strength of the bonding surface and uniformly transfer the load, the bonding surfaces between the layers are consistent with the direction of the spherical surface of the ball tooth, and the curvature of each bonding surface decreases from top to bottom and is embedded in the bonding surface of the previous layer, and the thickness of each transition layer gradually increases.

[0021] In this embodiment, the specific steps for preparing the stacked carbide ball gear are as follows: Step 1: Preparation of high hardness layer material (1) The hard phase is composed of recycled fine WC powder with a particle size of 1.5 μm and Co powder with a particle size of 1 μm, wherein the mass fraction of the recycled fine WC powder is 94% and the mass fraction of the Co powder is 6%. When preparing the hard phase, the recycled fine WC powder and the Co powder are wet-milled, the wet-milling medium is alcohol, and the wet-milling time is 32 h. After the wet-milling, spray drying is performed. After drying, the mixed powder is loaded into a tubular furnace for high-temperature calcination. The calcination temperature is 1050 ° C and the calcination time is 2.5 h. Finally, the mixed powder after calcination and cooling is sieved to obtain the hard phase; (2) The matrix phase is composed of coarse WC powder with a particle size of 7 μm and Co powder with a particle size of 1 μm, wherein the mass fraction of the coarse WC powder is 90% and the mass fraction of the Co powder is 10%. The coarse WC powder and the Co powder are wet-milled with alcohol as the wet milling medium for 20 h. After the wet milling, the mixed slurry is sieved to obtain the matrix phase. (3) 70% by weight of the hard phase and 30% by weight of the matrix phase were fully mixed at 55°C for 3 hours, paraffin was added as a molding agent during the mixing, and the amount of paraffin added was 3% of the total weight of the hard phase and the matrix phase. After being fully mixed, the mixture was dried at 85°C in a vacuum drying oven for 2.5 hours, and then sieved and granulated to finally obtain a high hardness layer material; (4) In order to ensure that the high hardness layer has sufficient wear resistance and strength, the thickness of the high hardness layer is set to 5 mm; Step 2: Preparation of high-toughness layer material (1) The high-toughness layer material is a two-layer transition layer material, which is composed of coarse WC powder with a particle size of 7 μm and Co powder with a particle size of 1 μm. The coarse WC powder and Co powder are wet-milled, and the wet-milling medium is alcohol. The wet-milling time is 22 h. After the wet-milling, they are dried at 85 °C in a vacuum drying oven for 2.5 h, and then sieved and granulated to obtain the high-toughness layer material; (2) To ensure that the high-toughness layer has sufficient bending strength, fracture toughness, uniform stress distribution and can evenly transfer load, the mass fraction of coarse WC in each transition layer from top to bottom is 88% and 86% respectively; the mass fraction of Co powder is 12% and 14% respectively, and the thickness of the transition layer is prepared at a ratio of 1:1.5, where the thickness of the first transition layer is set to 4 mm; Step 3: Forming and sintering of laminated carbide ball gear materials The prepared high-hardness layer material and high-toughness material are powdered layer by layer and then pressed to obtain a pressed green body, which is then sintered in a low-pressure sintering furnace at 1410°C for 1.5 hours and a sintering pressure of 6MPa. After sintering, a stacked cemented carbide ball gear material can be obtained. The properties of the stacked cemented carbide material prepared by the above process are shown in Table 1.

[0022] Example 3 Referring to Example 1, the preparation method of this embodiment is the same as that of Example 1, except that in this embodiment, the mass percentage of the hard phase is 50%, the mass percentage of the matrix phase is 50%, and after the mixture is pressed and sintered, a stacked cemented carbide material is obtained, and its test performance is shown in Table 1.

[0023] Comparative Example 1 The cemented carbide material of this comparative example is composed of a single homogeneous microstructure consisting of coarse WC powder with a particle size of 7μm and Co powder with a particle size of 1μm, wherein the mass fraction of the coarse WC powder is 90%, and the mass fraction of the Co powder is 10%. During preparation, the coarse WC powder and the Co powder are wet-milled, the wet-milling medium is alcohol, and the wet-milling time is 22h. After the wet-milling, the mixture is dried at 85°C in a vacuum drying oven for 2.5h, and then sieved and granulated to obtain a cemented carbide mixture. The mixture is pressed into a green body, and then sintered at 1410°C in a low-pressure sintering furnace for 1.5h and a sintering pressure of 6MPa. After the sintering, a cemented carbide ball gear material is obtained, and its test properties are shown in Table 1.

[0024] Comparative Example 2 The cemented carbide material of this comparative example is composed of a single homogeneous microstructure consisting of 1.5μm recycled WC powder, 1μm Co powder and Y2O3. The mass fraction of recycled WC is 89.5%; the mass fraction of Co powder is 10%; and the mass fraction of Y2O3 is 0.5%. The recycled WC powder, Co powder and fully dissolved Y(NO3)3 solution are wet-milled with alcohol as the wet-milling medium for 32 hours, followed by drying. The dried mixed powder is then loaded into a tubular furnace for high-temperature calcination at 850°C for 1.5 hours. Finally, the calcined mixed powder is sieved to obtain a cemented carbide mixture. The mixture is pressed into a green body, and then sintered at 1410°C in a low-pressure sintering furnace for 1.5 hours and a sintering pressure of 6MPa. After sintering, a cemented carbide ball tooth material is obtained, and its test properties are shown in Table 1.

[0025] Table 1 shows the properties of the cemented carbide button materials in Examples 1 to 3 and Comparative Examples 1 to 2 It can be seen from Table 1 that the laminated cemented carbide button gear material has excellent comprehensive mechanical properties. The high-hardness layer takes into account the high hardness of the hard phase and the high toughness of the matrix phase, so that the high-hardness layer exhibits better comprehensive properties such as wear resistance and impact resistance; the high-toughness layer has higher fracture toughness, so that the high-toughness layer exhibits better fracture resistance. Therefore, the laminated cemented carbide button gear material can significantly improve the service life and efficiency in harsh environments, and reduce manufacturing and maintenance costs.

[0026] Depend on Figures 2-3 The microstructure diagrams of the stacked cemented carbide high hardness layer at different magnifications of Example 1 show that the hard phase maintains a complete spherical structure and is evenly distributed in the matrix phase. Since the hard phase has high hardness and the matrix phase has high toughness, the high hardness layer has both high hardness and high toughness.

[0027] Figure 4This is the organizational structure diagram of the interface between the high-hardness layer and the high-toughness layer of the stacked cemented carbide in Example 1. It can be seen from the figure that the interface between the high-hardness layer and the high-toughness layer is well bonded, and cracking between the layers is not likely to occur. In addition, the high-toughness layer is a single homogeneous microstructure and therefore has higher toughness and strength.

[0028] The present invention solves the problem that it is difficult to take both the hardness and fracture toughness of traditional homogeneous cemented carbide into account by combining a high-hardness layer material with a high-toughness layer material; the design combining multiple layers and a special structure helps to increase the contact area and bonding strength between layers, which can ensure that the alloy transfers loads evenly during application, improve the impact buffering effect, and solve the problems of gradient layer performance mutation and stress concentration of traditional gradient cemented carbide; recycled WC powder is used as the hard phase material, and the strengthening phase is doped with solid and liquid to ensure the uniformity of the strengthening phase distribution, improve the comprehensive performance of the recycled WC powder, and greatly reduce the preparation cost; the stacked cemented carbide material and ball tooth prepared by the present invention have both high wear resistance and high impact resistance, which solves the problems of fast wear, poor durability and high cost of ordinary ball tooth materials in the prior art, and significantly improves the service life and efficiency of cemented carbide under complex and harsh working conditions.

Claims

1. A method for preparing low-cost laminated cemented carbide button teeth for mining. Features: The following steps are involved: Step 1: Preparation of high hardness layer material (1) The hard phase consists of recycled fine WC powder, Co powder and Y 2 O 3 The hard phase is prepared by mixing regenerated fine WC powder, Co powder and fully dissolved Y(NO 3 ) 3 The solution is wet-milled and spray-dried, and then the mixed powder is calcined in a tube furnace. After the mixed powder is cooled to room temperature, it is graded and sieved to obtain a hard phase; (2) The matrix phase is composed of coarse WC powder and Co powder. The matrix phase is prepared by wet grinding the coarse WC powder and Co powder and then sieving to obtain the matrix phase; (3) The hard phase and the matrix phase are uniformly mixed according to the corresponding configuration ratio, so that the hard phase is evenly distributed in the matrix phase, thereby obtaining a high hardness layer material; Step 2: Preparation of high-toughness layer material (1) The high-toughness layer material is composed of coarse WC powder and Co powder. When preparing the high-toughness layer material, the coarse WC powder and Co powder are wet-grinded, and then dried and sieved to obtain the high-toughness layer material; (2) The high-toughness layer material is composed of at least two layers of transition layer materials, in which the thickness of each transition layer gradually increases from top to bottom, and the Co content of each layer also increases from top to bottom; Step 3: Forming and sintering of laminated carbide ball gears The prepared high-hardness layer material and high-toughness material are powdered layer by layer and then pressed to obtain a pressed green body, which is then sintered in a low-pressure sintering furnace to obtain a stacked cemented carbide ball gear material.

2. A method for preparing a low-cost laminated cemented carbide button for mining as claimed in claim 1, Features: In the raw materials for preparing the hard phase in step 1, the mass fraction of Co is 5%-8%, and the mass fraction of Y 2 O 3 The mass fraction is 0%-1%, and the balance is recycled fine WC powder. The particle size of the recycled WC powder is 1-2μm, the particle size of the Co powder is 1-2μm, and the Y(NO 3 ) 3 The purity is 99.9%, Y 2 O 3 is through Y(NO 3 ) 3 Obtained by thermal decomposition.

3. A method for preparing a low-cost laminated cemented carbide button for mining as claimed in claim 1, Features: When preparing the hard phase in step 1, the calcination temperature is 850°C-1100°C, the calcination time is 1-3h, and after the calcination, it is cooled to room temperature, wherein the heating rate is 10°C / min, and the cooling rate is 10°C / min.

4. A method for preparing a low-cost laminated cemented carbide button for mining as claimed in claim 1, Features: In the raw materials for preparing the matrix phase in step 1, the mass fraction of Co is 8%-10%, and the remainder is coarse WC powder, the particle size of the coarse WC powder is 4-8 μm, and the particle size of the Co powder is 1-2 μm.

5. A method for preparing a low-cost laminated cemented carbide button for mining as claimed in claim 1, Features: In the step 1, the hard phase and the matrix phase are mixed by heating and mechanical stirring, the heating temperature is 50-60° C., and the mixing time is 2-6 hours.

6. A method for preparing a low-cost laminated cemented carbide button for mining as claimed in claim 1, Features: In the step 1, the mass percentage of the hard phase added is 50%-80%, the mass percentage of the matrix phase added is 20%-50%, and the amount of the molding agent added is 2%-4% of the total weight of the hard phase and the matrix phase.

7. A method for preparing a low-cost laminated cemented carbide button for mining as claimed in claim 1, Features: In the step 1, the thickness of the high hardness layer material is ≥4 mm.

8. A method for preparing a low-cost laminated cemented carbide button for mining as claimed in claim 1, Features: In the step 2, the mass fraction of Co in the high-toughness layer material is 10%-14%, and the remainder is coarse WC. The particle size of the coarse WC powder is 4-8 μm, and the particle size of the Co powder is 1-2 μm.

9. A method for preparing a low-cost laminated cemented carbide button for mining as claimed in claim 1, Features: In the step 2, the thickness of the high-toughness layer material is ≥8 mm, and the ratio of the thickness of the transition layer is 1:1.

5.

10. A method for preparing a low-cost laminated cemented carbide button for mining as claimed in claim 1, Features: In the step three, the sintering temperature is 1410-1460° C., the sintering time is 1-2 h, and the sintering pressure is ≥5 MPa.