Preparation method of Bi (at) CNT sodium ion battery negative electrode material with excellent cycle performance and high rate performance
By combining carbon nanotubes with -COOH and Bi3+, Bi@CNT composite materials were prepared, which solved the performance problems caused by Bi volume changes in sodium-ion batteries, achieved high rate and excellent cycle performance, and significantly improved the performance of sodium-ion batteries. electrochemical performance and application value.
Patent Information
- Application Number
- CN202410714674.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
AI Technical Summary
Sodium-ion batteries have limited energy density, poor rate capability, and poor cycle stability, mainly due to the lack of anode materials that can provide a medium voltage platform, high theoretical specific capacity, significant rate performance, and long cycle life, especially the volume of metal bismuth during cycling. Large changes lead to electrode crushing and SEI film damage, affecting battery performance.
Carbon nanotubes with -COOH are combined with Bi3+, and micron-sized Bi@CNT composites are prepared through high-temperature treatment to simplify the synthesis process, establish strong interface connections, suppress the volume expansion of Bi and improve conductive properties.
It has achieved excellent cycle performance and high rate performance of Bi@CNT sodium-ion battery anode material, with a maximum reversible capacity of 450-470mAh/g, a capacity retention rate of 94%-97% after 5000 cycles, and 3300 cycles under high load. There is still a specific discharge capacity of 260-280mAh/g, which significantly improves the sodium storage capacity and structural stability.
Smart Images

Figure CN118720155A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sodium ion battery negative electrode materials and relates to a method for preparing a Bi@CNT sodium ion battery negative electrode material with excellent cycle and high rate performance. Background Art
[0002] Sodium-ion batteries (SIBs) are expected to become an alternative technology to lithium-ion batteries due to their abundant resources and low cost. Although SIBs have made some significant progress, their limited energy density, poor rate capability, and poor cycling stability are prominent obstacles to practical application. The main challenge is largely the lack of anode materials that can provide a medium voltage platform, high theoretical specific capacity, significant rate performance, and long cycle life. In general, it is generally believed that the voltage platform and high theoretical specific capacity are related to the elemental composition of the material, while the rate performance and cycling stability mainly depend on the electronic conductivity and structural stability of the material.
[0003] In the field of negative electrode materials, people have explored many negative electrode materials, such as carbon materials, metal materials, transition metal oxides, sulfides, phosphides, titanium-based compounds and fluorides. Among them, metallic bismuth is regarded as a promising negative electrode material for sodium ion batteries due to its high theoretical specific capacity (386mAh / g) and moderate working potential (0.5-0.75V). However, as a negative electrode material, the volume change of metallic bismuth during the cycle of sodium ion batteries is as high as 250%. On the one hand, this will cause serious electrode crushing and shedding of active materials on the current collector, resulting in interruption of electron transfer and rapid capacity decay of the entire battery. On the other hand, it will cause continuous destruction and repair of the SEI film, resulting in irreversible electrolyte consumption and high charge transfer resistance. Both will cause the continuous deterioration of the capacity of Bi electrode materials.
[0004] In order to improve the deterioration of the volume and capacity of sodium-ion batteries, many strategies have been successfully developed to improve the electrochemical properties of bismuth by designing various nanostructures and using carbon materials as conductive matrices. According to previous studies, combining conductive carbonaceous materials with Bi to design new nanostructures is considered to be an effective method to improve its electrochemical performance. For example, (J. Mater. Chem. A, 2021, 9, 22364) Li et al. synthesized Bi nanosheet microspheres with an open-pore structure, which had a high capacity of 361 mAh / g after 10,000 cycles at a current density of 5 A / g. (J. Mater. Chem. A, 2021, 9, 22048) The nitrogen-doped carbon-coated bismuth nanoparticle composite prepared by Chen et al. showed excellent cycle stability and still had a capacity of 326.9 mAh / g after 5,000 cycles at 2 A / g. (Nano Lett., 2019, 19, 1998–2004.) Yu's group synthesized a bismuth nanorod composite wrapped in N-doped carbon nanotubes, which had a high capacity of 302 mAh / g after 1000 cycles at a current density of 1 A / g. (Chem Asian J. 2021, 16, 2314-2320) Ma et al. prepared a N-doped carbon-wrapped Bi nanoflower composite material, which still had a reversible specific capacity of 363 mAh / g after 4000 cycles at a current density of 2 A / g. However, in such Bi / C composites, it is still a huge challenge to fully utilize the active materials, provide abundant active sites and sufficiently high theoretical electrochemical capacity, and provide sufficient and strong interfacial electronic connections between the active materials and the nanoscale carbon matrix to ensure high-throughput transmission of electrons / ions. In addition, the synthesis process of some materials is complicated or requires additional auxiliary reagents, resulting in low yield and high cost, which hinders their application. Therefore, distributing the active material Bi on the carbon matrix and establishing a strong interface connection between them through a simple synthetic route will be very promising to improve the electrochemical performance of bismuth-based anodes and have certain practical application value. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a Bi@CNT sodium ion battery negative electrode material with excellent cycle and high rate performance, using a CNT material with -COOH and Bi 3+ Combined with the above, a Bi@CNT composite material with a micron size is obtained after high-temperature treatment, which effectively suppresses the volume expansion problem of Bi alone as a negative electrode material for sodium ion batteries, improves the conductivity of the Bi@CNT composite material, reduces the polarization phenomenon when used as a sodium ion negative electrode material, and enhances the high-rate performance of the Bi@CNT electrode material.
[0006] To achieve the above object, the present invention is implemented through the following technical solutions:
[0007] A method for preparing a Bi@CNT sodium ion battery negative electrode material with excellent cycle and high rate performance comprises the following steps:
[0008] 1) Weigh 1-4 g of Bi(NO)3·5H2O and add it to 20-80 mL of alcohol solution. Stir magnetically for 0.5-3 h to completely dissolve the solid matter.
[0009] 2) adding 0.05-0.3 g of carbon nanotubes with -COOH to the solution obtained in step 1), stirring for 0.5-4 h to form a uniform suspension solution, then transferring the suspension solution into a polytetrafluoroethylene container, and reacting the solution in a high pressure reactor at 150-200° C. for 6-16 h;
[0010] 3) After cooling to room temperature, the reaction liquid was filtered with deionized water and ethanol, and the obtained black solid was placed in a drying oven at 80±5°C and dried for 12 to 16 hours;
[0011] 4) The dried sample is heated to 500-1000°C at 2-6°C / min in a tube furnace under an inert atmosphere, and maintained at 500-1000°C for 0.5-4h, and then cooled.
[0012] The alcohol solution is one of ethylene glycol, propylene glycol, butylene glycol and isopropanol.
[0013] The outer wall diameter of the carbon nanotube is 20-30nm, the length of the carbon nanotube is 0.5-2μm, and the carbon nanotube is a 2-3-layer multi-walled carbon nanotube.
[0014] The Bi@CNT sodium ion battery negative electrode material obtained by cooling in step 4) has a maximum reversible capacity of 450-470 mAh / g at a current density of 0.2 A / g after being assembled into a battery; the capacity retention rate is 94%-97% after 5000 cycles at a current density of 10 A / g, and the capacity retention rate is 1.33 mg / cm at a current density of 50 A / g. 2 After 3300 cycles, the discharge specific capacity is 260-280 mAh / g.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] The preparation method of Bi@CNT sodium ion battery negative electrode material only uses simple hydrothermal and high temperature treatment, the preparation process is relatively simple, and the material source is abundant. 3+Combined with the above, a Bi@CNT composite material with a micron size is obtained after high-temperature treatment, which effectively suppresses the volume expansion problem of Bi alone as a negative electrode material for sodium ion batteries, and the introduction of CNT effectively improves the conductivity of the Bi@CNT composite material. The sodium ion battery prepared with it has a maximum reversible capacity of 450-470mAh / g at a current density of 0.2A / g (much higher than the theoretical specific capacity of 386mAh / g). After 5000 cycles at a current density of 10A / g, the capacity retention rate is 94% to 97%. And at a current density of 50A / g, the loading amount is 1.33mg / cm 2 After 3300 cycles, it still has a discharge specific capacity of 260-280 mAh / g, which is much higher than the sodium storage capacity of Bi@C composite materials reported in recent years, achieving efficient and ultra-stable sodium storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the preparation flow chart of Bi@CNT sodium-ion battery negative electrode material.
[0018] Figure 2 This is the XRD diagram of Bi@CNT sodium-ion battery negative electrode material.
[0019] Figure 3 This is the SEM image of the Bi@CNT sodium-ion battery negative electrode material;
[0020] Figure 3 Middle: (a), (b), and (c) are SEM images at different magnifications.
[0021] Figure 4 This is the XPS image of Bi@CNT sodium-ion battery anode material;
[0022] Figure 4 In the figure: (a) is the full spectrum of Bi@CNT material; (b) is the Bi 4f fine spectrum of Bi@CNT material; (c) is the O1s fine spectrum of Bi@CNT material; (d) is the C1s fine spectrum of Bi@CNT material.
[0023] Figure 5 This is the cycle performance diagram of Bi@CNT sodium-ion battery negative electrode material after 100 cycles at a current density of 0.2A / g.
[0024] Figure 6 This is the cycle performance diagram of Bi@CNT sodium-ion battery negative electrode material after 2200 cycles at a current density of 5A / g.
[0025] Figure 7 This is the cycling performance diagram of Bi@CNT sodium-ion battery negative electrode material at a current density of 10A / g.
[0026] Figure 8 This is the cycling performance diagram of Bi@CNT sodium-ion battery negative electrode material at a current density of 50A / g.
[0027] Fig. 9 This is the rate performance diagram of Bi@CNT sodium-ion battery negative electrode material at different current densities.
[0028] Fig.10 This is the impedance spectrum of Bi@CNT sodium-ion battery negative electrode material. DETAILED DESCRIPTION
[0029] The present invention is described in detail below in conjunction with the accompanying drawings, but it should be noted that the implementation of the present invention is not limited to the following embodiments.
[0030] See Figure 1 A method for preparing a Bi@CNT sodium ion battery negative electrode material with excellent cycle and high rate performance comprises the following steps:
[0031] 1) Weigh 1-4 g of Bi(NO)3·5H2O and add it to 20-80 mL of alcohol solution, and stir magnetically for 0.5-3 h to completely dissolve the solid matter; the alcohol solution is one of ethylene glycol, propylene glycol, butylene glycol, and isopropanol.
[0032] 2) Add 0.05-0.3 g of carbon nanotubes with -COOH to the solution obtained in step 1), stir for 0.5-4 h to form a uniform suspension solution, then transfer it into a 100 ml polytetrafluoroethylene container and react in a high pressure reactor at 150-200 ° C for 6-16 h; the outer wall diameter of the carbon nanotubes is 20-30 nm, the length of the carbon nanotubes is 0.5-2 μm, and they are 2-3 layers of multi-walled carbon nanotubes.
[0033] 3) After cooling to room temperature, the reaction liquid was filtered with deionized water and ethanol, and the obtained black solid was placed in a drying oven at 80±5°C and dried for 12 to 16 hours;
[0034] 4) The dried sample is heated to 500-1000°C at 2-6°C / min in a tube furnace under an inert atmosphere, and maintained at 500-1000°C for 0.5-4h, and then cooled.
[0035] The obtained Bi@CNT sodium ion battery negative electrode material was assembled into a battery, which had a maximum reversible capacity of 450-470 mAh / g at a current density of 0.2 A / g; the capacity retention rate was 94%-97% after 5000 cycles at a current density of 10 A / g, and the capacity retention rate was 1.33 mg / cm at a current density of 50 A / g. 2After 3300 cycles, the discharge specific capacity is 260-280 mAh / g.
[0036] Example
[0037] See Figure 1 , a method for preparing Bi@CNT sodium ion battery negative electrode material with excellent cycle and high rate performance:
[0038] First, 2g Bi(NO)3·5H2O was dissolved in 50ml ethylene glycol and magnetically stirred at room temperature for 1h until there was no solid matter. Then 0.1g carbon nanotubes (CNT) with -COOH were added to the solution and stirred for 3h until a uniform suspension solution was formed. Then it was transferred into a 100ml polytetrafluoroethylene container and reacted at 180℃ in an autoclave for 12h. After the reaction was complete, the autoclave was allowed to cool naturally to room temperature. The obtained solution was filtered with a suction flask. Deionized water and anhydrous ethanol were added several times during the filtration process to obtain a black solid. Finally, the dried sample was heated to 800℃ at a heating rate of 5℃ / min in a tube furnace filled with nitrogen atmosphere and kept at a constant temperature of 800℃ for 2h.
[0039] Depend on Figure 2 It can be seen that the spectrum corresponds to the standard card ICDD No. 01-085-1329, indicating that the Bi@CNT material was successfully prepared.
[0040] Figure 3 This is the SEM image of the sample prepared in Example 1. There are several unique structures in the Bi@CNT material. One is Bi balls with a diameter of micrometers. The second is that a large number of CNTs are grown on these Bi balls. The third is that some nanoscale Bi particles are wrapped by CNTs. Since the carbonized CNT material has very excellent conductive properties, it can provide a good electron transmission channel for the main material Bi. The presence of CNTs can also improve the transmission of ions in the main material Bi, thereby enhancing the high-rate capability of Bi.
[0041] See Figure 4 From the full spectrum, we can see that there are C (284.6eV), O (531.3eV) and Bi (Bi5d26.08eV, Bi5p 102.08eV, Bi4f 159-165eV, Bi4d 442.08eV, Bi4p 532.08eV) elements in Bi@CNT material. Figure 4 There are two strong peaks in the HRXPS spectrum of Bi 4f in (b), located at 160.7 and 164.9 eV, corresponding to Bi 4f 7 / 2 and Bi 4f 5 / 2orbital, the peaks at 159.6 eV and 166.1 eV correspond to the formation of Bi-O bonds, indicating that the Bi surface is partially oxidized. Figure 4 From the O1s fine spectrum in (c), we can see that the peaks at 530.1, 531.8 and 533.3 eV correspond to CO / C=O, CO-Bi and Bi-O-Bi bonds. The existence of Bi-O-Bi indicates that there is a small amount of bismuth oxide in the Bi@CNT material, and the existence of CO-Bi proves that there is a certain link between Bi and the CNT interface, which promotes the rapid ion / electron transfer between Bi and the CNT matrix during the electrochemical process, thereby enhancing the rapid charge and discharge capability of the material. In addition, Figure 4 In the HRXPS spectrum of C1s in (d), three peaks located at 284.6, 285.6, and 290.5 eV can be observed, corresponding to CC, CO, and C=O bonds, respectively.
[0042] Depend on Figure 5 It can be seen that when the current density of the Bi@CNT electrode material is 0.2A / g, it still has a reversible capacity of 462mAh / g after 100 cycles.
[0043] Depend on Figure 6 It can be seen that the Bi@CNT electrode material still has a reversible capacity of 377.6 mAh / g after 2200 cycles at 5 A / g.
[0044] Depend on Figure 7 It can be seen that the Bi@CNT electrode material has a conductivity of 0.99, 1.22 and 1.36 mg / cm at 10 A / g. 2 The capacities were 329.5, 335.5 and 338.9 mAh / g after 2600, 2000, and 1490 cycles with different loading amounts, respectively.
[0045] Depend on Figure 8 It can be seen that the Bi@CNT electrode material has a conductivity of 0.89 and 1.33 mg / cm at 50 A / g. 2 The capacities were 248.1 and 277.3 mAh / g after 5000 and 3300 cycles with different loading amounts, respectively.
[0046] Depend on Fig. 9 It can be seen that the capacity of Bi@CNT electrode material has almost no attenuation before the current density of 10A / g, indicating that Bi@CNT material has excellent structural stability. When the current density gradually increases to 50A / g and returns to 0.1A / g, the capacity does not decrease significantly compared with the just-discharged state, indicating that the material has very excellent rate performance, which is due to its good conductivity.
[0047] Depend on Fig.10It can be seen that the charge transfer impedance of the Bi@CNT electrode material is 0.72Ω, which shows that the Bi@CNT electrode material has very excellent conductive properties.
[0048] This example successfully constructed a high-performance, low-cost Bi@CNT sodium-ion battery anode material. Thanks to the unique structure of the composite material, Bi@CNT has a higher reversible capacity than the theoretical capacity of Bi metal, with a reversible capacity of 0.99, 1.22 and 1.36 mg / cm at 10 A / g. 2 The loading capacity of the electrolyte was 329.5, 335.5 and 338.9 mAh / g after 2600, 2000 and 1490 cycles respectively. In addition, even at a current density of 50 A / g, the capacity of the electrolyte was 0.89 and 1.33 mg / cm 2 The capacity of the battery is still 248.1 and 277.3 mAh / g after 5000 and 3300 cycles respectively, which has considerable practical application value.
Claims
1. A method for preparing a Bi@CNT sodium ion battery negative electrode material with excellent cycle and high rate performance, It is characterized in that The following steps are involved: 1) Weigh 1-4g of Bi(NO) 3 ·5H 2 O is added to 20-80 mL of alcohol solution and stirred magnetically for 0.5-3 h to completely dissolve the solid matter; 2) adding 0.05-0.3 g of carbon nanotubes with -COOH to the solution obtained in step 1), stirring for 0.5-4 h to form a uniform suspension solution, then transferring the suspension solution into a polytetrafluoroethylene container, and reacting the solution in a high pressure reactor at 150-200° C. for 6-16 h; 3) After cooling to room temperature, the reaction liquid was filtered with deionized water and ethanol, and the obtained black solid was placed in a drying oven at 80±5°C and dried for 12 to 16 hours; 4) The dried sample is heated to 500-1000°C at 2-6°C / min in a tube furnace under an inert atmosphere, and maintained at 500-1000°C for 0.5-4h, and then cooled.
2. A method for preparing a Bi@CNT sodium ion battery negative electrode material having excellent cycle and high rate performance according to claim 1, It is characterized in that The alcohol solution is one of ethylene glycol, propylene glycol, butylene glycol and isopropanol.
3. A method for preparing a Bi@CNT sodium ion battery negative electrode material having excellent cycle and high rate performance according to claim 1, It is characterized in that The outer wall diameter of the carbon nanotube is 20-30nm, the length of the carbon nanotube is 0.5-2μm, and the carbon nanotube is a 2-3-layer multi-walled carbon nanotube.
4. A method for preparing a Bi@CNT sodium ion battery negative electrode material having excellent cycle and high rate performance according to claim 1, It is characterized in that The Bi@CNT sodium ion battery negative electrode material obtained by cooling in step 4) is assembled into a battery and has a maximum reversible capacity of 450-470 mAh / g at a current density of 0.2 A / g; The capacity retention rate is 94% to 97% after 5000 cycles at a current density of 10 A / g, and the loading capacity is 1.33 mg / cm 2 After 3300 cycles, the discharge specific capacity is 260-280 mAh / g.