Unequal-thickness TIG (Tungsten Inert Gas) welding method for 22MnB5 and QStE550TM high-strength steel

Through the TIG welding method, the deformation problem when welding dissimilar high-strength steel plates of unequal thickness is solved, high-quality welding formation and full penetration are achieved, the welding cost and deformation are reduced, and the tensile strength of the joint is ensured.

CN118720346APending Publication Date: 2024-10-01PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411072693.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to specify appropriate welding parameters for the welding of dissimilar high-strength steels, resulting in defects such as burn-through or incomplete penetration, which affects the normal service of the welded joints, especially when welding thin plates of unequal thickness, which is prone to local deformation.

Method used

Using TIG welding method, the welding side of QStE550TM high-strength steel is processed to the same thickness as 22MnB5 high-strength steel, and double-sided welding is performed. The welding parameters are set to welding current 60~65A, voltage 12~14V, and wire feed speed 200mm·min. -1, use pure argon gas protection, flame preheating to prevent cold cracks, and vertical welding in a double-sided welding process.

Benefits of technology

It achieves good forming of high-strength steel sheets with unequal thickness, reduces welding heat input, reduces welding deformation, ensures full penetration of welded joints, smooth welded plate shape, improves welding quality, and reaches the tensile strength of the base metal in the tensile test .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720346A_ABST
    Figure CN118720346A_ABST
Patent Text Reader

Abstract

The invention relates to an unequal-thickness TIG welding method for 22MnB5 and QStE550TM high-strength steel. The unequal-thickness TIG welding method comprises the steps that S1, the welding side of the QStE550TM high-strength steel is machined to be the same as the 22MnB5 high-strength steel in thickness; s2, the 22MnB5 high-strength steel and the QStE550TM high-strength steel are in butt joint and fixed; s3, the butt joint of the two kinds of high-strength steel and the nearby area are cleaned; s4, selecting a welding wire; s5, TIG welding process parameters are set; s6, the two kinds of high-strength steel are preheated, and cold cracks are prevented; and S7, the welding gun is perpendicular to the surface of the plate to be welded, and welding is conducted. According to the method, the 22MnB5 and QStE550TM dissimilar high-strength steel is welded through the TIG welding process, TIG welding forming of the thin plate can be achieved, and the problem of connector deformation during welding of the thin plates with different thicknesses is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-strength steel welding, and in particular to a TIG welding method for 22MnB5 and QStE550TM high-strength steels with unequal thicknesses. Background Art

[0002] Due to its high strength, corrosion resistance, good formability and weldability, high-strength steel is widely used in automobile manufacturing, offshore platforms, petrochemicals, aerospace and other fields. Reasonable combination of dissimilar high-strength steels can give full play to the advantages and performance of the two steels to achieve the purpose of saving precious metals, which has practical significance for reducing production costs.

[0003] However, since the two high-strength steels may have large differences in chemical composition and physical properties, this brings great difficulty to the welding of dissimilar steels. It is more common in the welding of dissimilar steels that it is difficult to specify appropriate welding parameters due to the large difference in melting points of the two steels, which often results in defects such as burn-through or incomplete penetration, affecting the normal service of the welded joint. Therefore, the selection of welding methods and the formulation of welding parameters are extremely important for the connection of dissimilar steels.

[0004] At present, when welding dissimilar steels, especially high-strength steel sheets of unequal thickness, local deformation is prone to occur during welding due to the influence of welding heat input and the difficulty in beveling, thus affecting the normal use of the welded joint. Summary of the invention

[0005] In view of the above problems, the purpose of the present invention is to provide a TIG welding method for 22MnB5 and QStE550TM high-strength steels of unequal thickness. For 22MnB5 and QStE550TM dissimilar high-strength steels, TIG welding process is used for welding, which can realize TIG welding forming of thin plates and effectively improve problems such as joint deformation during welding of thin plates of unequal thickness.

[0006] The technical solution adopted by the present invention is as follows:

[0007] The present invention proposes a 22MnB5 and QStE550TM high-strength steel unequal thickness TIG welding method, which specifically comprises the following steps:

[0008] S1. Process the welding side of QStE550TM high-strength steel to the same thickness as 22MnB5 high-strength steel;

[0009] S2. Butt and fix the 22MnB5 high-strength steel and the QStE550TM high-strength steel;

[0010] S3. Clean the joints of the two high-strength steels and the surrounding areas;

[0011] S4, select welding wire;

[0012] S5. Setting TIG welding process parameters;

[0013] S6. Preheat the two high-strength steels to prevent cold cracks;

[0014] S7. Place the welding gun perpendicular to the surface of the plate to be welded and perform welding.

[0015] Furthermore, in step S1, the thickness of QStE550TM high-strength steel is higher than that of 22MnB5 high-strength steel, and a groove structure with a slope of 30° is processed on the welding side of QStE550TM high-strength steel so that the thickness of its welding side is the same as that of 22MnB5 high-strength steel.

[0016] Furthermore, the step S3 specifically includes: removing dirt, scale, labels and paint within 30 mm from the joint of the two steel plates and the surrounding area, and polishing with sandpaper to reveal the metallic luster, and wiping the cleaned area with anhydrous ethanol after polishing.

[0017] Furthermore, in step S4, the welding wire is H08Mn2Si welding wire with a diameter of 1.1-1.3 mm.

[0018] Furthermore, in step S5, the TIG welding process parameters are: welding current 60-65A, welding voltage 12-14V, wire feeding speed 200mm·min -1 , the protective gas is pure argon.

[0019] Furthermore, in step S6, the preheating method is flame preheating, the preheating temperature is 80-100°C, and the temperature of the plate to be welded is heated to a specified temperature before subsequent operations are performed.

[0020] Furthermore, in step S7, the welding adopts a double-sided welding process. After completing the welding of one side, the slag inclusions on the back side of the welding plate are cleaned, and then the welding of the other side is continued.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The TIG double-sided welding process adopted by the present invention can greatly reduce the welding heat input for high-strength steel sheets of unequal thickness while ensuring good welding joint formation, thereby reducing welding costs and welding deformation.

[0023] (2) The double-sided welding process of the present invention realizes full penetration of the weld while maintaining a smooth weld plate shape and minimal welding deformation.

[0024] (3) The present invention performs welding preheating treatment on the high-strength steel plate to prevent cold cracks from occurring during welding, thereby improving the welding quality.

[0025] In the tensile test of the dissimilar steel joints of the present invention, the tensile strength of the joints can reach the tensile strength of the parent material QStE550TM high-strength steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The figure is a schematic flow chart of a TIG welding method for unequal thickness of 22MnB5 and QStE550TM high-strength steels proposed in the present invention.

[0027] Figure 2 It is a schematic diagram of the welding groove structure of 22MnB5 and QStE550TM dissimilar high-strength steels in the present invention. DETAILED DESCRIPTION

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] See attached Figure 1 The present invention proposes a 22MnB5 and QStE550TM high-strength steel unequal thickness TIG welding method, which specifically includes the following steps:

[0030] S1. Process the welding side of QStE550TM high-strength steel to the same thickness as 22MnB5 high-strength steel; wherein the thickness of QStE550TM high-strength steel is greater than that of 22MnB5 high-strength steel, and process a groove structure with a slope of 30° on the welding side of QStE550TM high-strength steel, such as Figure 2 As shown, the thickness of its welding side is the same as that of the welding side of 22MnB5 high-strength steel.

[0031] S2. Butt and fix the 22MnB5 high-strength steel and QStE550TM high-strength steel.

[0032] S3. Clean the joints of the two high-strength steels and the surrounding areas, including: removing dirt, scale, labels and paint within 30 mm of the joints of the two steel plates and the surrounding areas, and polishing with sandpaper to reveal the metallic luster. After polishing, wipe the cleaned area with anhydrous ethanol.

[0033] S4. Select welding wire: Use H08Mn2Si welding wire with a diameter of 1.1-1.3mm.

[0034] S5. Set TIG welding process parameters: welding current 60-65A, welding voltage 12-14V, wire feeding speed 200mm·min -1 , the protective gas is pure argon.

[0035] S6. Preheat the two high-strength steels with flames at a temperature of 80 to 100°C. After the plates to be welded are heated to the specified temperature, subsequent operations can be carried out to prevent cold cracks.

[0036] S7. The welding gun is perpendicular to the surface of the plate to be welded, and a double-sided welding process is adopted. After completing the welding on one side, clean the slag on the back of the welded plate, and then continue to weld the other side.

[0037] The present invention will be further described below by means of specific embodiments:

[0038] Example 1

[0039] The thickness of the 22MnB5 high-strength steel plate used is 2mm, the tensile strength is 1550MPa, and the yield strength is 1216MPa; the thickness of the QStE550TM high-strength steel plate is 2.8mm, the tensile strength is 643MPa, and the yield strength is 561MPa. Using the welding method of the present invention, the welding wire uses a 1.2mm diameter H08Mn2Si welding wire.

[0040] The welding method includes the following steps:

[0041] S1. Process a groove structure with a slope of 30° on the welding side of QStE550TM high-strength steel so that the thickness of its welding side is the same as that of the welding side of 22MnB5 high-strength steel;

[0042] S2. Butt and fix the 22MnB5 high-strength steel and the QStE550TM high-strength steel;

[0043] S3. Clean the joints of the two high-strength steels and the surrounding areas;

[0044] S4, select welding wire;

[0045] S5. Set TIG welding parameters; welding current 65A, welding voltage 14V, wire feeding speed 200mm·min -1 , the protective gas is pure argon.

[0046] S6. flame preheating the two high-strength steels at a preheating temperature of 80°C;

[0047] S7. The welding gun is perpendicular to the surface of the welding plate and double-sided welding process is used for welding.

[0048] The process requirements after welding are:

[0049] There are no defects such as collapse, pores and cracks on the weld surface, and the weld root is fully melted.

[0050] In the tensile test of the welded dissimilar steel joints, the tensile strength of the welded joints is not less than that of QStE550TM high-strength steel.

[0051] Example 2

[0052] The thickness of the 22MnB5 high-strength steel plate used is 1.8 mm, the tensile strength is 1543 MPa, and the yield strength is 1209 MPa; the thickness of the QStE550TM high-strength steel plate is 2.2 mm, the tensile strength is 633 MPa, and the yield strength is 507 MPa. When using the welding method of the present invention, the welding wire uses H08Mn2Si welding wire.

[0053] The welding method includes the following steps:

[0054] S1. Process a groove structure with a slope of 30° on the welding side of QStE550TM high-strength steel so that the thickness of its welding side is the same as that of the welding side of 22MnB5 high-strength steel;

[0055] S2. Butt and fix the 22MnB5 high-strength steel and the QStE550TM high-strength steel;

[0056] S3. Clean the joints of the two high-strength steels and the surrounding areas;

[0057] S4, select welding wire;

[0058] S5. Set TIG welding parameters: welding current 60A, welding voltage 12V, wire feeding speed 200mm·min -1 , the protective gas is pure argon.

[0059] S6. Preheating the two high-strength steels at a preheating temperature of 100°C;

[0060] S7. The welding gun is perpendicular to the surface of the welding plate and double-sided welding process is used for welding.

[0061] The process requirements after welding are:

[0062] There are no defects such as collapse, pores and cracks on the weld surface, and the weld root is fully melted.

[0063] In the tensile test of the welded dissimilar steel joints, the tensile strength of the welded joints is not less than that of QStE550TM high-strength steel.

[0064] The working principle of the present invention is:

[0065] By adopting the method of preheating before welding, the cooling rate of the weld joint is reduced, thereby avoiding the generation of hardened phase inside the weld joint, reducing welding stress, removing residual stress in the steel plate processing process, and improving the deformation problem of the weld joint.

[0066] By adopting the low heat input method, the comprehensive heat input of the weld joint is reduced, the microstructure composition and grain size of the weld zone and the heat-affected zone are controlled, thereby reducing the proportion of martensite in the weld zone and improving the plasticity of the weld joint.

[0067] The two-pass welding process of front and back welding is adopted. The temperature field of the back welding tempers the front welding, so that the martensite in the weld area is transformed into tempered martensite and bainite, etc., thereby effectively eliminating the hardened structure and improving the toughness of the welded joint.

[0068] Matters not described in detail in the present invention are all known technologies.

[0069] The embodiments described above are merely descriptions of preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A TIG welding method for 22MnB5 and QStE550TM high-strength steel of unequal thickness, characterized in that: The method comprises the following steps: S1. Process the welding side of QStE550TM high-strength steel to the same thickness as 22MnB5 high-strength steel; S2. Butt and fix the 22MnB5 high-strength steel and the QStE550TM high-strength steel; S3. Clean the joints of the two high-strength steels and the surrounding areas; S4, select welding wire; S5. Setting TIG welding process parameters; S6. Preheat the two high-strength steels to prevent cold cracks; S7. Place the welding gun perpendicular to the surface of the plate to be welded and perform welding.

2. The method for TIG welding of 22MnB5 and QStE550TM high-strength steel of unequal thickness according to claim 1, characterized in that: In the step S1, the thickness of QStE550TM high-strength steel is higher than that of 22MnB5 high-strength steel, and a groove structure with a slope of 30° is processed on the welding side of QStE550TM high-strength steel so that the welding side has the same thickness as that of 22MnB5 high-strength steel.

3. The method for TIG welding of 22MnB5 and QStE550TM high-strength steel of unequal thickness according to claim 1, characterized in that: The step S3 specifically includes: removing dirt, scale, labels and paint within 30 mm of the joint of the two steel plates and the surrounding area, and polishing with sandpaper to expose the metallic luster, and wiping the cleaned area with anhydrous ethanol after polishing.

4. The method for TIG welding of 22MnB5 and QStE550TM high-strength steel of unequal thickness according to claim 1, characterized in that: In step S4, the welding wire is H08Mn2Si welding wire with a diameter of 1.1-1.3 mm.

5. The method for TIG welding of 22MnB5 and QStE550TM high-strength steel of unequal thickness according to claim 1, characterized in that: In step S4, the TIG welding process parameters are: welding current 60-65A, welding voltage 12-14V, wire feeding speed 200mm·min -1 , the protective gas is pure argon.

6. The method for TIG welding of 22MnB5 and QStE550TM high-strength steel of unequal thickness according to claim 1, characterized in that: In step S6, the preheating method is flame preheating, the preheating temperature is 80-100°C, and the subsequent operation is carried out after the temperature of the plate to be welded is heated to the specified temperature.

7. The method for TIG welding of 22MnB5 and QStE550TM high-strength steel of unequal thickness according to claim 1, characterized in that: In step S7, the welding adopts a double-sided welding process. After completing the welding of one side, the slag inclusions on the back side of the welding plate are cleaned, and then the welding of the other side is continued.