Cover surface surfacing material for surfacing composite manufacturing of roll surfaces of steel rolling rolls, pinch rolls and wrapper rolls and preparation method and surfacing process of cover surface surfacing material

By optimizing the composition of C, Mn, Si, Cr, V+Nb, Mo+Co, Zr+Ti in the cladding materials and encapsulating protective mineral granulation technology, combined with the annealing heat treatment process, we have solved the problem of existing cladding materials in The problem of insufficient thermal stability and thermal fatigue resistance at high temperatures has been achieved, achieving higher service life and cost reduction.

CN118720525AInactive Publication Date: 2024-10-01BEIJING NEW VISION BUILDING CONSTR TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410877502.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing cladding materials are difficult to meet the thermal stability, thermal fatigue resistance and wear resistance requirements of rolling rollers, pinch rollers, and coil-assist rollers at high temperatures, resulting in short service life and high consumption costs.

Method used

The cover surfacing material is used to contain deposited metal with specific components, including C, Mn, Si, Cr, V+Nb, Mo+Co, Zr+Ti, and the mineral granulation is protected by optimizing the weight percentage and wrapping of these elements. technology to improve the hardness, thermal stability and oxidation resistance of the material, and adopt an annealing heat treatment process.

Benefits of technology

It significantly improves the high-temperature hardness, oxidation resistance and thermal fatigue performance of the cladding material, extends the service life, reduces the roll consumption cost, and solves the problem of steel sticking and cracks, leaving the surface smooth and defect-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720525A_ABST
    Figure CN118720525A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of surfacing, and discloses a capping surfacing material for surfacing composite manufacturing of roll surfaces of a steel rolling roll, a pinch roll and a wrapper roll, and a preparation method and a surfacing process of the capping surfacing material. The deposited metal of the capping surfacing material comprises the following components in percentage by weight: 0.5%-1.5% of C, 0.5%-1.5% of Ni, 0.5%-1.5% of Ni, and the balance of Fe; 0.5% to 3.8% of Mn; 0.1% to 0.9% of Si; cr: 11.0% to 15.5%; 0.2%-2.8% of V + Nb; 0.50% to 2.5% of Mo + Co; 1%-6% of Zr + Ti; and the balance of Fe. The capping surfacing material disclosed by the invention is prepared by firstly coating the Zr + Ti alloy with protective mineral substances, granulating, and then mixing with other alloy compounds or alloy particles. The capping surfacing material provided by the invention has good thermal stability, and can improve the working performance of each roller at high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a surfacing material for composite manufacturing of rolling mill rolls, pinch rolls and auxiliary coiling rolls and a preparation method thereof, a surfacing process, and in particular to a cover surfacing material and a surfacing process for composite manufacturing and remanufacturing of various rolling mill rolls, pinch rolls and auxiliary coiling rolls of hot-rolled strip coilers, and belongs to the technical field of surfacing. Background Art

[0002] Rolling rolls, pinch rolls and coiling rolls are the most critical components of rolling and curling equipment. The bending moment and contact stress on the roll body during operation are generally smaller than the rolling moment and contact stress of other rolls on the same rolling line. Rolling rolls, pinch rolls and coiling rolls must be replaced during overhaul (once a year), and their surface temperature is generally 550℃~1150℃ during operation.

[0003] Composite welding is an important branch in the field of welding, mainly used in industries such as steel, cement, and electricity. How to obtain thermally stable cladding materials and perfect processes with good hardness, high-temperature wear resistance, thermal fatigue resistance, impact resistance, etc. is an important problem that plagues the welding industry. Summary of the invention

[0004] The purpose of the present invention is to provide a surfacing material for composite manufacturing of rolling mill rolls, pinch rolls and winding rollers, so as to meet the requirements of the rolls working at high temperatures of 550°C to 1150°C, have good thermal stability, increase service life and reduce roll consumption costs.

[0005] Another object of the present invention is to provide a method for preparing a cladding material for composite manufacturing of rolling mill rolls, pinch rolls and winding rollers.

[0006] Another object of the present invention is to provide a surfacing welding process for composite manufacturing of rolling mill rolls, pinch rolls and winding rollers.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] A surfacing welding material for composite manufacturing of rolling mill rollers, pinch rollers and winding rollers. The deposited metal of the surfacing welding material contains the following components by weight percentage: C: 0.5% to 1.5%; Mn: 0.5% to 3.8%; Si: 0.1% to 0.9%; Cr: 11.0% to 15.5%; V+Nb: 0.2% to 2.8%; Mo+Co: 0.50% to 2.5%; Zr+Ti: 1% to 6%; and the balance is Fe.

[0009] The main functions of the elements in the cap cladding material and cladding deposited metal are:

[0010] (1)C

[0011] The main function of C is to form a large number of fine and dispersed carbides with Mo, Ti, V, Cr, etc., which greatly improves the hardness, thermal stability, high-temperature wear resistance and other properties of the cladding metal. At the same time, C is also the main element that inhibits the formation of high-temperature ferrite. The present application optimizes the weight percentage of C to 0.5% to 1.5%, for example, 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, etc. A higher content of C can improve the weld hardness and annealing softening resistance of the cladding metal. More importantly, as the carbon content increases, the occurrence of steel sticking during the use of the roll is reduced, which is beneficial to the stability of the steel plate surface. When the C content is too low, for example, less than 0.45%, the steel sticking phenomenon is more serious, causing the roll to be offline prematurely.

[0012] (2)Cr

[0013] The increase of chromium content increases the hardenability, oxidation resistance and corrosion resistance of the deposited metal. Chromium not only forms chromium carbide with carbon but also can solid solution strengthen the matrix. Therefore, the hardness of the cladding deposited metal is improved while improving the oxidation resistance.

[0014] (3) Mo, V, Nb, Co

[0015] Optimizing a certain amount of vanadium and niobium through thermal fatigue experiments can improve thermal fatigue performance; through oxidation experiments and high-temperature hardness experiments, it was found that a certain amount of molybdenum and cobalt can significantly improve the oxidation resistance and red hardness of the surfacing alloy. Further, optimizing the weight percentage of V+Nb to 0.2%~2.8% can more effectively improve thermal fatigue performance. Optimizing the weight percentage of Mo+Co to 0.50%~2.5% can more significantly improve the oxidation resistance and red hardness of the surfacing alloy.

[0016] (4) Zr+Ti

[0017] Zr+Ti purifies the deposited metal and has a metamorphic effect, improving the high-temperature strength, high-temperature plasticity and oxidation resistance of the weld, which is beneficial to improving the high-temperature application performance.

[0018] Furthermore, the weight percentage of Zr+Ti is optimized (increased) to 1% to 6%, for example, 1%, 2%, 3%, 4%, 5%, 6%, etc. A higher content of Zr+Ti can reduce the risk of welding cracks on the one hand, and on the other hand, it is conducive to combining with carbon to form dense carbides to reduce the probability of steel sticking, that is, there is no sticky slag on the surface during use, the light and dark stripes are not obvious, and the surface is smooth. When the Zr+Ti content is too low, for example, the content is ≤0.8%, it is not conducive to the control of cracks and the reduction of the probability of steel sticking.

[0019] In addition, the cap surfacing material in the present invention is prepared by first granulating the Zr+Ti alloy to protect the minerals, and then mixing with other alloy compounds or alloy particles. The present invention uses zirconium and titanium to strengthen the surfacing material, first granulating the Zr+Ti externally to protect the minerals, reducing the burning of Zr+Ti, while refining the grains and improving the organizational properties; then mixing the powders and making the cap surfacing material according to the normal process, such as the finished flux-cored welding wire.

[0020] In the manufacturing process of the cover welding material, in order to ensure the smooth transition of Zr+Ti, reduce the burning loss of Zr+Ti and refine the grains, and improve the organizational properties, the Zr+Ti alloy is specially wrapped and protected by mineral granulation. Optionally, the following steps are used for processing:

[0021] 1) mixing a Zr+Ti alloy with carbonate, borate and graphite to obtain a mixed material;

[0022] 2) adding potassium sodium mixed water glass to the mixed material and stirring thoroughly;

[0023] 3) sending the stirred wet powder into a granulator for granulation;

[0024] 4) After granulation, dry, crush and make granules.

[0025] The main purposes of granulation by the above steps are: 1. To prevent severe burning and increase the transition coefficient; 2. To refine the grains and improve the organizational properties.

[0026] Furthermore, carbonate, borate and graphite, which are 5 to 40% of the total weight of the Zr+Ti alloy, are mixed with the Zr+Ti alloy, and then potassium sodium mixed water glass is added. Furthermore, the mass ratio of carbonate, borate and graphite is 10:1 to 10:0.1 to 1. By using the above-mentioned specific mineral materials to wrap the Zr+Ti alloy and controlling the amount of components, the Zr+Ti alloy can be better transitioned into the weld and reduce oxidation during the molten pool process; on the other hand, the wrapped Zr+Ti alloy is conducive to improving the nucleation rate and the refinement of the structure. Therefore, the Zr+Ti alloy after effective wrapping effectively reduces the burnout of Zr+Ti while improving the grain refinement effect and improving the structure performance.

[0027] The carbonate may be, for example, potassium carbonate, sodium carbonate, calcium carbonate, lithium carbonate, barium carbonate, etc., and the borate may be, for example, potassium fluoroborate, sodium fluoroborate, barium fluoroborate, etc.

[0028] Optionally, the particle sizes of the carbonate, borate and graphite are all -100 mesh.

[0029] Optionally, the particle size of the Zr+Ti alloy is -60 to +160 mesh (meaning that the particle size is smaller than the aperture of a sieve within the range of 60 to 100 mesh).

[0030] Optionally, after granulation, the granules are dried in a drying furnace at 150° C. to 250° C. for 0.5 to 1.5 hours, for example, at 200° C. for about 1 hour, and then crushed to form granules of -40 to 100 mesh.

[0031] Optionally, the concentration of the potassium-sodium mixed water glass (also called potassium-sodium water glass) is 18-20%.

[0032] Optionally, in the cap surfacing material, Zr is added in the form of zirconium silicon alloy, and Ti is added in the form of titanium iron, and the addition amount of the two meets 1:0.5 to 1. Based on the weight percentage of Zr+Ti being 1% to 6%, optimizing the addition ratio of the two can better control the generation of cracks under different carbon and different alloy contents, and at the same time help reduce the occurrence of steel sticking during use.

[0033] Furthermore, in the cap surfacing material, the deposited metal structure is annealed troostite, and carbides are distributed on the austenite matrix.

[0034] Wherein, when the cover surface cladding material is used for cladding composite manufacturing, the cover surface cladding material has the following properties:

[0035] Hardness of deposited metal in welded state: ≥56HRc

[0036] Hardness after annealing at 580℃: ≥55HRc

[0037] There are no defects such as cracks after welding.

[0038] A method for preparing a cover cladding material for manufacturing a rolling mill roll, a pinch roll, or a winding roller by cladding composite manufacturing according to the present invention comprises:

[0039] The Zr+Ti alloy is wrapped to protect the minerals and granulated to obtain granulated particles;

[0040] The granulated particles are mixed with other alloy compounds or alloy particles according to the weight percentage of each component in the deposited metal of the capping welding material to prepare the capping welding material.

[0041] For example, after mixing, the cladding material is made according to conventional processes, for example, after being wrapped with a steel strip, it is drawn into a finished welding wire, such as a flux-cored welding wire with a diameter of Φ3.2 mm.

[0042] A surfacing process for composite manufacturing of rolling mill rolls, pinch rolls and auxiliary rolls by surfacing welding using the surfacing welding material, in which annealing heat treatment is performed after surfacing welding using the surfacing welding material. By improving the traditional tempering heat treatment to annealing heat treatment, it is more conducive to the stability of high-temperature microstructure performance.

[0043] Optionally, the surfacing process may include the following steps:

[0044] (1) Preheating: The preheating temperature is 220-280°C, for example 260°C.

[0045] Further optionally, during preheating, within the range of room temperature to 100°C, the heating rate is not higher than 40°C / h; after exceeding 100°C, the heating rate is not higher than 50°C / h, and the heating is uniform.

[0046] (2) Requirements for cladding parameters: Taking Φ3.2mm flux-cored welding wire as an example, for Φ3.2mm flux-cored welding wire, the requirements are:

[0047] Welding current: 450~480A;

[0048] Welding voltage: 27V~32V;

[0049] Welding speed: 380mm / min~500mm / min;

[0050] Weld overlap: The overlap of adjacent welds must be greater than 50%. The specific overlap amount should be determined by the smoothness of the weld.

[0051] Welding polarity: DC reverse connection;

[0052] Wire extension length: 16mm~28mm;

[0053] Weld interlayer temperature: 260℃~380℃.

[0054] (3) After welding, the rolling rollers, pinch rollers and auxiliary winding rollers are heat treated at a temperature of 300°C to 350°C for 1h to 2h; they are slowly cooled to room temperature at a cooling rate of no more than 25°C / h.

[0055] (4) Annealing: The annealing temperature is 570-590°C, for example, 580°C, and the constant temperature time is not less than 4 hours.

[0056] (5) As the furnace temperature drops to 150°C, take the rolling rollers, pinch rollers, and auxiliary winding rollers out of the furnace and place them in a special box or cover them with asbestos to slowly cool them to room temperature.

[0057] Further optionally, during annealing, within 100°C, the heating rate is not less than 40°C / h, and then the heating rate is not less than 50°C / h; when cooling with the furnace, the cooling rate is not less than 25°C / h.

[0058] The advantages of the present invention are:

[0059] The present invention optimizes various components and their contents in the deposited metal of the cap cladding material through various experiments, thereby improving the high temperature performance of the cap cladding material.

[0060] The present invention firstly wraps the Zr+Ti externally to protect the mineral granulation, thereby reducing the burning loss of Zr+Ti, facilitating the smooth transition of Zr+Ti, improving the cost performance and further improving the oxidation resistance and high temperature hardness of the weld.

[0061] The present invention further improves the high-temperature strength of the surfacing material and the stability of the surfacing body structure by optimizing alloy elements, Zr+Ti externally wrapped and protected mineral granulation, and adopts an annealing heat treatment process, while being beneficial to high-temperature plasticity and oxidation resistance.

[0062] In addition, the cap surfacing material and surfacing process of the present invention have been successfully applied to the surfacing composite manufacturing of hot-rolled strip steel continuous rolling mill strip steel rolling rolls, pinch rolls, and auxiliary rolls. After being used on the machine, the surface has good anti-oxidation performance, no sticky slag on the surface, no obvious light and dark stripes, and a smooth surface. It can meet the working conditions of the rolls, and its service life is significantly improved compared with ordinary surfacing materials on the market, reducing the consumption cost of the rolls, and completely solving the problem of low service life of the steel rolling rolls, pinch rolls, and auxiliary rolls. In addition, the surfacing composite (re) manufacturing of hot-rolled working rolls of other rolling mills can also use the cap surfacing material and the corresponding surfacing process of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 A comparison diagram of the morphologies of Example 3 and the comparative example of the present invention after being used on the auxiliary winding roller of the same winding machine is shown. DETAILED DESCRIPTION

[0064] The following embodiments of the present invention are only used to illustrate the specific implementation methods of the present invention, rather than to limit the protection scope of the present invention. For those skilled in the art, various changes or modifications can be made without departing from the technical feature scope of the present invention. Their essence is the same as the technical solution of the present invention and all belong to the protection scope of the present invention.

[0065] Granulated Material Examples 1 to 4

[0066] Taking 1000 grams of Zr+Ti alloy, potassium carbonate, potassium fluoroborate and graphite as an example, the specific implementation is shown in Table 1:

[0067] Table 1 Mass of Zr+Ti powder, potassium carbonate, potassium fluoroborate and graphite

[0068]

[0069] After mixing in this proportion, add potassium sodium mixed with water glass of self-prepared concentration and stir thoroughly; send the stirred wet powder into a granulator for granulation; after granulation, dry it in a drying furnace at 200°C for about 1 hour; finally, crush it to make particles of -40 to 100 mesh.

[0070] Deposited Metal Examples 1 to 4

[0071] The above particles are used to design welding wires with the chemical composition shown in Table 2, and the particles are used together with other alloy particles to produce flux-cored welding wires. Performance tests are carried out after surfacing with the cap surfacing material.

[0072] Table 2 Mass percentage of each component in the cover welding material (wt%)

[0073]

[0074] Surfacing process:

[0075] 1) Preheat the rolls, and then, after preheating, weld the capping materials prepared in Examples 1 to 4 on the rolls (Φ400 mm×600 mm) whose base material is 45# steel.

[0076] During surfacing welding, two layers of low alloy base layers are firstly surfacing welded on the substrate, with a single-side surfacing thickness of about 5 mm, and then the cover surfacing materials in Examples 1 to 4 are surfacing welded, with a single-side surfacing thickness of 15 mm.

[0077] The specific process parameters of the cladding operation are shown in Table 3.

[0078] Table 3 Surfacing process parameters

[0079]

[0080] 2) After surfacing, continue to keep the temperature at 350℃ on the roller for 1h, then slowly cool to room temperature with a cooling rate of no more than 25℃ / h.

[0081] 3) Perform annealing heat treatment at 580°C for 10 hours; wherein, the heating process: from room temperature to less than 100°C, the heating rate is 40°C / h, and then the heating rate is 50°C / h; the cooling process: the cooling rate is 25°C / h, and then cools to room temperature.

[0082] 4) Finally, after magnetic powder and ultrasonic testing, the results showed that there were no defects such as cracks on the surface. The hardness was measured according to the national standard, and the results are shown in Table 4.

[0083] Table 4 Partial mechanical properties of the cap cladding materials of Examples 1 to 4 at different temperatures

[0084]

[0085] It can be seen from Table 4 above that the cap surfacing material prepared in the above embodiment of the present invention has a room temperature hardness of ≥58HRC and a hardness of ≥56.5HRc after annealing at 580°C, and the high temperature hardness of the material is improved.

[0086] In addition, the above-mentioned cover surfacing materials are used for composite surfacing to manufacture the strip rolling rollers, pinch rollers and winding auxiliary rollers of the hot-rolled strip continuous rolling mill. After being used on the machine, they have good surface oxidation resistance, no sticky slag on the surface, no obvious light and dark stripes, and a smooth surface. They can meet the working conditions of the rollers, and their service life is significantly increased compared with ordinary surfacing materials on the market, reducing the consumption cost of the rollers.

[0087] The following gives the usage of the roller machine corresponding to the cover welding material of Example 3 and the comparative example, and further analyzes the influence of the carbon and Zr+Ti content in the deposited metal formula of the cover welding material on the service life of the machine.

[0088] The difference between the comparative example and Example 3 is that the chemical composition reduces the carbon content to 0.45%, and the Zr+Ti content to 0.8%, while the other components remain unchanged and the preparation method is the same.

[0089] Figure 1 The morphology comparison diagram of Example 3 and the comparative example after using the auxiliary winding roller of the same winding machine is shown. Among them, Figure 1 (a) is a morphology image of Example 3 after the steel mill coiler auxiliary coiler coiled 600,000 tons. Figure 1 (b) is the morphology of the comparative example after the auxiliary winding roller of the same winding machine was used. Figure 1 (a) It can be seen that after the roller product corresponding to the material of Example 3 of the present application is used on the machine, the surface has good anti-oxidation performance, no sticky residue on the surface, no obvious light and dark stripes, and a smooth surface. Figure 1 (b) It can be seen that: when using the comparative material, after only curling 100,000 tons, the surface is seriously sticky. It can be seen that the material of the present application can meet the working conditions of the roller. The present application improves the high temperature strength, high temperature plasticity and oxidation resistance of the weld by Zr+Ti purification and modification, which is conducive to the improvement of high temperature application performance. Based on this effect, a higher content of Zr+Ti and a higher content of carbon are used to reduce the generation of cladding cracks and the occurrence of steel sticking.

[0090] The description of the present invention is given for the purpose of illustration and description, and is not intended to be exhaustive or to limit the invention to the disclosed form. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for particular uses.

Claims

1. A surfacing material for composite manufacturing of rolling mill rolls, pinch rolls, and winding rollers, characterized in that: The deposited metal of the cover welding material contains the following components in weight percentage: C: 0.5% to 1.5%; Mn: 0.5% to 3.8%; Si: 0.1% to 0.9%; Cr: 11.0% to 15.5%; V+Nb: 0.2% to 2.8%; Mo+Co: 0.50% to 2.5%; Zr+Ti: 1% to 6%; and the balance is Fe.

2. The cover welding material according to claim 1, characterized in that: The capping welding material is prepared by firstly wrapping the Zr+Ti alloy to protect the mineral granulation, and then mixing with other alloy compounds or alloy particles; The step of wrapping the Zr+Ti alloy to protect the mineral granulation includes: 1) Mixing Zr+Ti alloy with carbonate, borate and graphite to obtain a mixed material; wherein the amount of carbonate, borate and graphite is 5-40% of the total weight of the Zr+Ti alloy, and the mass ratio of the carbonate, borate and graphite is 10:1-10:0.1-1; 2) adding potassium sodium mixed water glass to the mixed material and stirring thoroughly; 3) sending the stirred wet powder into a granulator for granulation; 4) After granulation, the mixture is dried at 150°C to 250°C for 0.5 to 1.5 hours, and then crushed to form granules of -40 to 100 mesh.

3. The cap cladding material according to claim 2, characterized in that: The particle sizes of the carbonate, borate and graphite are all -100 mesh; the particle size of the Zr+Ti alloy is -60 to 160 mesh.

4. The cap cladding material according to claim 1, characterized in that: Zr is added in the form of zirconium silicon alloy, Ti is added in the form of ferrotitanium, and the addition amounts of the two satisfy 1:0.5-1.

5. The cap cladding material according to claim 1, characterized in that: When the cover cladding material is used for cladding composite manufacturing, the relevant performance parameters of the cladding deposited metal are: Hardness of deposited metal in welded state: ≥56HRc, Hardness after annealing at 580℃: ≥55HRc, No cracks after welding.

6. The cap cladding material according to claim 1, characterized in that: The deposited metal structure is annealed troostite, with carbides distributed on the austenite matrix.

7. A method for preparing a cover cladding material for manufacturing a rolling mill roll, a pinch roll, or a winding roller by cladding composite manufacturing according to any one of claims 1 to 6, characterized in that: include: The Zr+Ti alloy is wrapped to protect the minerals and granulated to obtain granulated particles; The granulated particles are mixed with other alloy compounds or alloy particles according to the weight percentage of each component in the deposited metal of the capping welding material to prepare the capping welding material.

8. A surfacing process for composite manufacturing of rolling mill rolls, pinch rolls and winding rollers using the surfacing material according to any one of claims 1 to 6, characterized in that: After surfacing welding with the cover surfacing material, annealing heat treatment is performed; The following steps are involved: 1) Preheating: The preheating temperature is 220-280°C; 2) Surfacing parameter requirements: Welding current: 450~480A; Welding voltage: 27V~32V; Welding speed: 380mm / min~500mm / min; Weld overlap: The overlap of adjacent welds must be greater than 50%; Welding polarity: DC reverse connection; Wire extension length: 16mm~28mm; Welding interlayer temperature: 260℃~380℃; 3) After welding, heat treatment is performed on the rolling rollers, pinch rollers and winding rollers at a temperature of 300°C to 350°C for 1h to 2h; they are slowly cooled to room temperature at a cooling rate of no more than 25°C / h; 4) Annealing: Annealing temperature is 570-590°C, and the constant temperature time is not less than 4h; 5) As the furnace temperature drops to 150°C, take the rolling rollers, pinch rollers and auxiliary winding rollers out of the furnace and place them in a special box or cover them with asbestos to slowly cool them to room temperature.

9. The surfacing welding process for composite manufacturing of rolling mill rolls, pinch rolls and winding rollers according to claim 8, characterized in that: During annealing, within 100°C, the heating rate shall not be less than 40°C / h, and thereafter the heating rate shall not be less than 50°C / h; when cooling with the furnace, the cooling rate shall not be less than 25°C / h.