Corrosion-resistant oak plate and preparation method thereof
By using preservatives such as dodecyldimethylbenzylammonium chloride and boron-containing compounds combined with hexamethylene diisocyanate and trimethoxy (3,3,3-trifluoropropyl)silane on oak boards, It solves the problems of oak board rot and insect damage in humid environment, achieves efficient and long-lasting anti-corrosion effect, and maintains the natural performance and environmental protection of wood.
Patent Information
- Application Number
- CN202410882878.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-03
AI Technical Summary
Oak boards are prone to rot, mildew, and insect infestation in humid environments. Existing preservatives are highly toxic and easily lost in humid environments, making it difficult to meet long-term anti-corrosion requirements.
Using dodecyldimethylbenzyl ammonium chloride and boron-containing compounds as the anti-corrosion main body, combined with hexamethylene diisocyanate and trimethoxy (3,3,3-trifluoropropyl) silane, through vacuum pressure The soaking process increases the hydrophobicity and durability of the preservative, forming a stable anti-corrosion barrier.
It significantly improves the long-term anti-corrosion effect of oak boards, extends its service life, maintains the natural beauty and mechanical properties of the wood, and has excellent environmental protection characteristics.
Abstract
Description
Technical Field
[0001] The invention relates to a wood board material, in particular to a corrosion-resistant oak board and a preparation method thereof. Background Art
[0002] Oak boards are widely used in construction and furniture manufacturing due to their excellent mechanical properties and beautiful texture. In addition, oak boards are also used to make wine barrels. Their unique wood structure and chemical composition can give the wine a unique flavor during the aging process. The porous structure of oak allows the wine to have a slight contact with the air, which promotes the maturation of the wine and the complexity of its flavor. However, oak boards are susceptible to rot, mildew and insect pests in a humid environment, which seriously affects their service life and structural strength. Therefore, effective antiseptic treatment of oak boards to improve their durability has become a technical problem that needs to be solved urgently.
[0003] Existing wood preservation technology usually relies on the use of chemical preservatives to prevent wood from rotting, mildew and insect infestation in humid environments. Although traditional preservatives such as CCA (copper chromium arsenate) and ACQ (alkylamine copper quaternary ammonium compound) have good antiseptic effects, they are highly toxic and pose potential hazards to the environment and human health, and some preservatives have been banned in Europe and North America. Therefore, the development of a safe, efficient and environmentally friendly wood preservative has become a research hotspot in the current technical field. These new preservatives need to provide long-term protection without causing harm to the environment and user health, while also maintaining the natural beauty and mechanical properties of the wood.
[0004] In recent years, researchers have found that boron-containing compounds have gradually become a new type of environmentally friendly preservatives due to their low toxicity and good anti-corrosion effects. These compounds include sodium fluoroborate, sodium metaborate and sodium tetraborate. Although boron-containing compounds have good anti-corrosion properties, they are easily soluble in water and easily lost in a humid environment, resulting in a weakened anti-corrosion effect. Therefore, relying solely on boron-containing compounds as preservatives is difficult to meet the anti-corrosion needs of wood in a long-term humid environment. Studies have shown that the solubility of boron-containing compounds in water not only affects their durability in wood, but may also have a negative impact on the anti-corrosion properties of wood, especially in wood applications that are often exposed to rain or high humidity environments.
[0005] In addition, recent studies have also found that dodecyl dimethyl benzyl ammonium chloride (DDBAC), which has broad-spectrum antibacterial, antifungal and insect-resistant effects, has also been used in wood preservation. DDBAC can effectively kill a variety of bacteria, fungi and insect pests. However, although DDBAC has a good antiseptic effect, its solubility in water also causes it to be easily lost in a humid environment, affecting its antiseptic performance.
[0006] Therefore, how to effectively reduce the loss of preservatives in a humid environment and improve their antiseptic effect and durability has become an urgent problem to be solved. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a corrosion-resistant oak board and a preparation method thereof, which has strong and lasting corrosion resistance.
[0008] The present invention aims to improve the anticorrosive properties of oak boards, and selects dodecyl dimethyl benzyl ammonium chloride with broad-spectrum antibacterial, antifungal and insect-proof effects, and sodium fluoroborate, sodium metaborate and sodium tetraborate etc. can provide boron-containing compounds of boron element as anticorrosive main raw materials. However, dodecyl dimethyl benzyl ammonium chloride and these boron-containing compounds are all soluble in water, causing them to be easily lost in a humid environment, affecting the anticorrosive effect. In order to overcome this problem, the present invention introduces hexamethylene diisocyanate and trimethoxy (3,3,3-trifluoropropyl) silane with high hydrophobicity. These components enhance its persistence and anti-loss performance in oak boards by improving the hydrophobicity of preservatives, thereby significantly improving the long-term anticorrosive effect of oak boards.
[0009] Specifically, the technical solution of the present invention is:
[0010] The invention provides a method for preparing a corrosion-resistant oak board, comprising soaking the oak board in a wood preservative liquid, wherein the wood preservative liquid comprises dodecyl dimethyl benzyl ammonium chloride and a boron-containing compound.
[0011] Preferably, the wood preservative liquid comprises the following raw materials in percentage by weight: 1-5 wt % of dodecyldimethylbenzyl ammonium chloride and 1-4 wt % of a boron-containing compound.
[0012] Preferably, the wood preservative liquid comprises the following raw materials in mass percentage: 2-4wt% dodecyldimethylbenzylammonium chloride and 2-3wt% boron-containing compound.
[0013] Preferably, the boron-containing compound is at least one of sodium fluoroborate, sodium metaborate and sodium tetraborate.
[0014] Preferably, the wood preservative solution further comprises hexamethylene diisocyanate and trimethoxy (3,3,3-trifluoropropyl) silane.
[0015] Preferably, the wood preservative liquid comprises the following raw materials in percentage by weight: 2-4 wt % dodecyldimethylbenzyl ammonium chloride, 2-3 wt % boron-containing compound, 0.2-0.8 wt % hexamethylene diisocyanate and 0.2-0.8 wt % trimethoxy (3,3,3-trifluoropropyl) silane.
[0016] Preferably, the wood preservative liquid comprises the following raw materials in mass percentage: 2-4wt% dodecyldimethylbenzyl ammonium chloride, 2-3wt% boron-containing compound, 0.2-0.8wt% hexamethylene diisocyanate, 0.2-0.8wt% trimethoxy (3,3,3-trifluoropropyl) silane, 0.5-1.5wt% surfactant, 3-7wt% ethanol, and the balance is water.
[0017] Preferably, the soaking step is a vacuum pressure soaking process.
[0018] Preferably, the vacuum pressure soaking process has a vacuum degree of 0.1-0.6Mpa and a soaking time of 60-120 minutes.
[0019] Preferably, the vacuum pressure soaking process is a two-stage vacuum pressure soaking process, wherein the first stage of the vacuum pressure soaking process has a vacuum degree of 0.1-0.3Mpa and a soaking time of 30-60 minutes; the second stage of the vacuum pressure soaking process has a vacuum degree of 0.4-0.6Mpa and a soaking time of 30-60 minutes.
[0020] The invention also provides a corrosion-resistant oak board, which is prepared by the method.
[0021] The present invention provides a corrosion-resistant oak board and a preparation method thereof. By using dodecyldimethylbenzyl ammonium chloride and a boron-containing compound with broad-spectrum antibacterial, anti-mildew and anti-insect effects as the main raw materials for wood antiseptic, and further introducing hexamethylene diisocyanate and trimethoxy (3,3,3-trifluoropropyl) silane, the hydrophobicity and chemical stability of the preservative are improved, and the long-term antiseptic effect of the oak board is significantly improved. DETAILED DESCRIPTION
[0022] The invention discloses a method for preparing a corrosion-resistant oak board, which comprises a process of subjecting the oak board to vacuum pressure immersion in a wood preservative liquid.
[0023] The wood preservative liquid comprises the following raw materials in percentage by weight: 2-4wt% of dodecyldimethylbenzyl ammonium chloride, 2-3wt% of boron-containing compounds, 0.2-0.8wt% of hexamethylene diisocyanate, 0.2-0.8wt% of trimethoxy (3,3,3-trifluoropropyl) silane, 0.5-1.5wt% of surfactant, 3-7wt% of ethanol, and the balance is water.
[0024] The method for preparing the wood preservative comprises the following steps: mixing dodecyl dimethyl benzyl ammonium chloride, a boron-containing compound, a surfactant and water to obtain liquid A; mixing hexamethylene diisocyanate, trimethoxy (3,3,3-trifluoropropyl) silane and ethanol to obtain liquid B; and mixing liquid A with liquid B to obtain the wood preservative liquid.
[0025] Dodecyldimethylbenzylammonium chloride (DDBAC), CAS No.: 139-07-1, as the main preservative, has broad-spectrum antibacterial, antifungal and insect repellent effects. It can effectively inhibit the growth of microorganisms in wood and significantly improve the antiseptic properties of oak boards.
[0026] Boron compounds such as sodium fluoroborate, sodium metaborate and sodium tetraborate provide boron elements and play a role in anti-corrosion, insect repellency and mildew resistance. Its low toxicity and high efficiency make it an important component of environmentally friendly preservatives.
[0027] It is further found that the existing boron-containing compounds such as sodium fluoroborate, sodium metaborate and sodium tetraborate have poor long-term performance in corrosion protection due to their good water solubility. In order to fundamentally improve this technical defect, the present invention uses the water-insoluble boron-containing compound tridecyl borate as the main raw material for corrosion protection to replace sodium fluoroborate, sodium metaborate and sodium tetraborate. Tridecyl borate, English name Tris (decyl) borate, CAS number 20236-81-1.
[0028] Specifically, the wood preservative liquid contains the following raw materials in mass percentage: 2-4wt% dodecyl dimethyl benzyl ammonium chloride, 2-3wt% tridecyl borate, 0.2-0.8wt% hexamethylene diisocyanate, 0.2-0.8wt% trimethoxy (3,3,3-trifluoropropyl) silane, 0.5-1.5wt% surfactant, 3-7wt% ethanol, and the balance is water. Dodecyl dimethyl benzyl ammonium chloride, Tween 80 surfactant and water are mixed to obtain liquid A; tridecyl borate, hexamethylene diisocyanate, trimethoxy (3,3,3-trifluoropropyl) silane and ethanol are mixed to obtain liquid B; liquid A is gradually added to liquid B, stirring is maintained, and the mixture is evenly mixed to obtain the wood preservative liquid.
[0029] Hexamethylene diisocyanate (HDI), CAS No. 822-06-0, reacts with the hydroxyl groups in wood through its isocyanate groups to form stable carbamate bonds (-NH-CO-O-), which enhances the fixation and chemical stability of the preservative, forms a stable three-dimensional network structure, and improves the durability and anti-loss of the preservative.
[0030] Trimethoxy (3,3,3-trifluoropropyl) silane, CAS No. 429-60-7, reacts with the hydroxyl groups in wood to form siloxane bonds (Si-O-Si), which improves the adhesion of preservatives. Its trifluoropropyl structure increases the hydrophobicity of preservatives, forming a waterproof layer on the surface of wood to prevent the intrusion of moisture and foreign substances.
[0031] The surfactant helps disperse the water-insoluble components to form a uniform emulsion, ensuring the uniformity and stability of the preservative solution. Preferably, the surfactant is an amphoteric surfactant or a nonionic surfactant. Further preferably, the surfactant is a nonionic surfactant, such as Tween 20, Tween 80, dodecyl glucoside, AEO-3, AEO-7, AEO-9, NPEO-10, PEG-40 hydrogenated castor oil, Span 20, Span 40, Span 60, Span 80, etc. can be used.
[0032] Ethanol acts as a solvent, helping to dissolve and disperse the ingredients, improving the efficiency and effectiveness of the wood treatment.
[0033] Water acts as the primary solvent and medium, ensuring that the ingredients are evenly mixed and penetrate the wood effectively.
[0034] The wood preservative liquid significantly improves the antibacterial, anticorrosive, mildew-proof and durability of wood through the synergistic effect of multiple components. In particular, by introducing hexamethylene diisocyanate and trimethoxy (3,3,3-trifluoropropyl) silane, the fixation and hydrophobicity of the preservative are improved, and a stable three-dimensional network structure and a waterproof layer are formed, thereby effectively preventing the intrusion of moisture and foreign substances, extending the service life of the wood, and having excellent environmental protection characteristics.
[0035] A method for preparing a corrosion-resistant oak board comprises the following steps: subjecting the oak board to a vacuum pressure soaking process in a wood preservative liquid.
[0036] The vacuum pressure soaking process is a two-stage vacuum pressure soaking process, wherein the first stage of the vacuum pressure soaking process has a vacuum degree of 0.1-0.3Mpa and a soaking time of 30-60 minutes; the second stage of the vacuum pressure soaking process has a vacuum degree of 0.4-0.6Mpa and a soaking time of 30-60 minutes.
[0037] The purpose of the first stage of vacuum pressure soaking process is to gradually remove the air inside the wood under low vacuum conditions, reduce the bubbles inside the wood, and prevent the wood from cracking during the subsequent pressurization process. This process can also allow the preservative liquid to initially enter the gaps between wood cells and tiny pores, and begin to evenly distribute the preservative liquid, laying the foundation for the full penetration of the preservative liquid under subsequent higher pressure.
[0038] The purpose of the second stage of vacuum pressure soaking process is to further deepen the penetration of the preservative liquid under higher vacuum conditions, and to force the preservative liquid into the deep cells and smaller pores of the wood to ensure the uniform distribution of the preservative liquid inside the wood. This process improves the fixation of the preservative, allowing the preservative liquid to penetrate deeply into the wood, thereby significantly enhancing the antiseptic effect and durability of the wood. Through high-pressure penetration, the preservative liquid forms a uniform and stable antiseptic barrier inside the wood, maximizing the service life of the wood.
[0039] Preferably, the mass ratio of the oak board to the wood preservative liquid is 1:(5-100).
[0040] After the vacuum pressure soaking process, the oak board is taken out and dried at 60-80° C., and the moisture content is controlled to be 8-12 wt % to obtain the corrosion-resistant oak board.
[0041] Embodiment 1:
[0042] The wood preservative liquid comprises the following raw materials in percentage by weight: 3 wt % of dodecyl dimethyl benzyl ammonium chloride, 2.5 wt % of boron-containing compound sodium tetraborate, and the balance is water.
[0043] The preparation method of the wood preservative comprises the following steps: mixing dodecyl dimethyl benzyl ammonium chloride, boron-containing compound sodium tetraborate and water at 30° C. to obtain the wood preservative liquid.
[0044] Embodiment 2:
[0045] The wood preservative liquid comprises the following raw materials in percentage by weight: 3 wt % of dodecyldimethylbenzyl ammonium chloride, 2.5 wt % of boron-containing compound sodium tetraborate, 1.0 wt % of hexamethylene diisocyanate, 0.8 wt % of Tween 80 surfactant, 5 wt % of ethanol, and the balance is water.
[0046] The preparation method of the above-mentioned wood preservative comprises the following steps: mixing dodecyl dimethyl benzyl ammonium chloride, a boron-containing compound sodium tetraborate, a Tween 80 surfactant and water at 30°C to obtain a liquid A; mixing hexamethylene diisocyanate and ethanol at 30°C to obtain a liquid B; gradually adding the liquid A to the liquid B, keeping stirring, and mixing evenly at 30°C to obtain the wood preservative liquid.
[0047] Embodiment 3:
[0048] The wood preservative liquid comprises the following raw materials in percentage by weight: 3 wt % of dodecyldimethylbenzyl ammonium chloride, 2.5 wt % of boron-containing compound sodium tetraborate, 1.0 wt % of trimethoxy (3,3,3-trifluoropropyl) silane, 0.8 wt % of Tween 80 surfactant, 5 wt % of ethanol, and the balance is water.
[0049] The preparation method of the above-mentioned wood preservative comprises the following steps: uniformly mixing dodecyldimethylbenzyl ammonium chloride, a boron-containing compound sodium tetraborate, a Tween 80 surfactant and water at 30°C to obtain a liquid A; uniformly mixing trimethoxy(3,3,3-trifluoropropyl)silane and ethanol at 30°C to obtain a liquid B; gradually adding the liquid A to the liquid B, keeping stirring, and uniformly mixing at 30°C to obtain the wood preservative liquid.
[0050] Embodiment 4:
[0051] The wood preservative liquid comprises the following raw materials in percentage by weight: 3 wt % of dodecyldimethylbenzyl ammonium chloride, 2.5 wt % of boron-containing compound sodium fluoroborate, 0.5 wt % of hexamethylene diisocyanate, 0.5 wt % of trimethoxy (3,3,3-trifluoropropyl) silane, 0.8 wt % of Tween 80 surfactant, 5 wt % of ethanol, and the balance is water.
[0052] The preparation method of the above-mentioned wood preservative comprises the following steps: uniformly mixing dodecyldimethylbenzyl ammonium chloride, a boron-containing compound sodium fluoroborate, a Tween 80 surfactant and water at 30°C to obtain a liquid A; uniformly mixing hexamethylene diisocyanate, trimethoxy (3,3,3-trifluoropropyl) silane and ethanol at 30°C to obtain a liquid B; gradually adding the liquid A to the liquid B, keeping stirring, and uniformly mixing at 30°C to obtain the wood preservative liquid.
[0053] Embodiment 5:
[0054] The wood preservative liquid comprises the following raw materials in percentage by weight: 3 wt % of dodecyldimethylbenzyl ammonium chloride, 2.5 wt % of boron-containing compound sodium metaborate, 0.5 wt % of hexamethylene diisocyanate, 0.5 wt % of trimethoxy (3,3,3-trifluoropropyl) silane, 0.8 wt % of Tween 80 surfactant, 5 wt % of ethanol, and the balance is water.
[0055] The preparation method of the above-mentioned wood preservative comprises the following steps: uniformly mixing dodecyldimethylbenzyl ammonium chloride, a boron-containing compound sodium metaborate, a Tween 80 surfactant and water at 30°C to obtain a liquid A; uniformly mixing hexamethylene diisocyanate, trimethoxy (3,3,3-trifluoropropyl) silane and ethanol at 30°C to obtain a liquid B; gradually adding the liquid A to the liquid B, keeping stirring, and uniformly mixing at 30°C to obtain the wood preservative liquid.
[0056] Embodiment 6:
[0057] The wood preservative liquid comprises the following raw materials in percentage by weight: 3 wt % of dodecyldimethylbenzyl ammonium chloride, 2.5 wt % of boron-containing compound sodium tetraborate, 0.5 wt % of hexamethylene diisocyanate, 0.5 wt % of trimethoxy (3,3,3-trifluoropropyl) silane, 0.8 wt % of Tween 80 surfactant, 5 wt % of ethanol, and the balance is water.
[0058] The preparation method of the above-mentioned wood preservative comprises the following steps: uniformly mixing dodecyldimethylbenzyl ammonium chloride, a boron-containing compound sodium tetraborate, a Tween 80 surfactant and water at 30°C to obtain a liquid A; uniformly mixing hexamethylene diisocyanate, trimethoxy (3,3,3-trifluoropropyl) silane and ethanol at 30°C to obtain a liquid B; gradually adding the liquid A to the liquid B, keeping stirring, and uniformly mixing at 30°C to obtain the wood preservative liquid.
[0059] Embodiment 7:
[0060] The wood preservative liquid comprises the following raw materials in percentage by weight: 3 wt % of dodecyldimethylbenzyl ammonium chloride, 2.5 wt % of boron-containing compound tridecyl borate, 0.5 wt % of hexamethylene diisocyanate, 0.5 wt % of trimethoxy (3,3,3-trifluoropropyl) silane, 0.8 wt % of Tween 80 surfactant, 5 wt % of ethanol, and the balance is water.
[0061] The preparation method of the above-mentioned wood preservative comprises the following steps:
[0062] Dodecyl dimethyl benzyl ammonium chloride, Tween 80 surfactant and water are mixed uniformly at 30°C to obtain liquid A; boron-containing compounds tridecyl borate, hexamethylene diisocyanate, trimethoxy (3,3,3-trifluoropropyl) silane and ethanol are mixed uniformly at 30°C to obtain liquid B; liquid A is gradually added to liquid B, stirring is maintained, and the mixture is mixed uniformly at 30°C to obtain the wood preservative liquid.
[0063] Application Examples 1-7:
[0064] A method for preparing a corrosion-resistant oak board:
[0065] Drying the oak board at 80° C. to a moisture content of 10 wt % to obtain a dried oak board;
[0066] The dried oak board was placed in the wood preservative liquid of Example 1-7 at 20 times its weight, and two vacuum pressure soaking processes were performed continuously.
[0067] The first stage of vacuum pressure soaking process: vacuum degree 0.2Mpa, 28℃ soaking time 50 minutes;
[0068] The second stage of vacuum pressure soaking process: vacuum degree 0.5Mpa, 28℃ soaking time 50 minutes;
[0069] After the two-stage vacuum pressure soaking process is completed, the oak board is taken out and dried at 75° C., and the final moisture content is controlled to be 10 wt % to obtain the corrosion-resistant oak board.
[0070] Application example 1 corresponds to the wood preservative liquid of embodiment 1, application example 2 corresponds to the wood preservative liquid of embodiment 2, and so on.
[0071] Application Example 8:
[0072] A method for preparing a corrosion-resistant oak board:
[0073] Drying the oak board at 80° C. to a moisture content of 10 wt % to obtain a dried oak board;
[0074] The dried oak board was placed in the wood preservative liquid of Example 6 at a weight 20 times that of the board, and a vacuum pressure soaking process was performed, with a vacuum degree of 0.35 MPa, a soaking time of 100 minutes at 28° C.;
[0075] After the vacuum pressure soaking process is completed, the oak board is taken out and dried at 75° C. to control the final moisture content to 10 wt % to obtain the corrosion-resistant oak board.
[0076] Application Example 9:
[0077] A method for preparing a corrosion-resistant oak board:
[0078] Drying the oak board at 80° C. to a moisture content of 10 wt % to obtain a dried oak board;
[0079] Place a dried oak board in the wood preservative liquid of Example 6 at 20 times its weight and immerse it at 28° C. for 100 minutes;
[0080] After the soaking process is completed, the oak board is taken out and dried at 75° C. to control the final moisture content to 10 wt % to obtain the corrosion-resistant oak board.
[0081] Test Example 1:
[0082] The anti-corrosion performance is tested according to "GB / T 13942.1-2009 Durability of Wood Part 1: Laboratory Test Method for Natural Corrosion Resistance".
[0083] Take 20mm×20mm×10mm oak boards treated with the wood preservative liquids of Application Examples 1-7, species: white oak, origin: United States, test strain: Gloeophyllum trabeum (Pers.) Murrill (strain number: CFCC86617), culture chamber temperature: 28°C, culture chamber relative humidity: 80%.
[0084] The mass loss rate of the wood sample before and after decay is calculated to judge the corrosion resistance of the sample. The lower the mass loss rate, the better the corrosion resistance of the material; the higher the mass loss rate, the worse the corrosion resistance of the material.
[0085] The blank sample was oak that was not treated with wood preservative liquid.
[0086] Table 1: Oak board anticorrosion performance test table
[0087] Sample mass loss rate (%) Application Example 1 14.71 Application Example 2 8.94 Application Example 3 8.16 Application Example 4 6.38 Application Example 5 7.54 Application Example 6 4.22 Application Example 7 2.67 Application Example 8 5.68 Application Example 9 8.83 Blank example 28.94
[0088] The anticorrosion performance of Example 6 is better than that of Example 2 and Example 3. Hexamethylene diisocyanate reacts with hydroxyl groups in wood through its isocyanate group to form a stable carbamate bond. This reaction not only enhances the fixation of the preservative, but also forms a stable three-dimensional network structure, which significantly improves the durability and anti-loss of the preservative. Trimethoxy (3,3,3-trifluoropropyl) silane reacts with hydroxyl groups in wood through its trimethoxy group to form a siloxane bond, thereby improving the adhesion of the preservative. At the same time, its trifluoropropyl structure increases the hydrophobicity of the preservative, forming a waterproof layer on the surface of the wood, effectively preventing the intrusion of moisture and foreign substances. Hexamethylene diisocyanate and trimethoxy (3,3,3-trifluoropropyl) silane provide chemical stability and physical barriers respectively by enhancing the fixation and hydrophobicity of the preservative. The synergistic effect of the two significantly improves the anticorrosion effect and durability of the wood, so that the preservative exhibits a more durable and efficient anticorrosion performance in a humid environment.
[0089] The anticorrosion performance of Example 6 is better than that of Example 4 and Example 5. Sodium tetraborate (Na2B4O7) is a polyborate with a high boron content and forms more stable boron compounds inside the wood. This polyborate not only performs well in anticorrosion, insect prevention and mildew prevention, but also its moderate solubility can effectively penetrate into the interior of the wood and is not easily lost in a humid environment. In contrast, although sodium fluoborate (NaBF4) contains fluorine, which can enhance the anticorrosion performance, its boron content is low, and the presence of fluorine may also increase its solubility and loss risk, thereby reducing the anticorrosion effect in a humid environment. Sodium metaborate (NaBO2), as a monoborate, has the lowest boron content and the highest solubility, so it loses faster in a humid environment and has a relatively weak anticorrosion effect.
[0090] On the whole, sodium tetraborate has high stability in wood and can form stronger chemical bonds with components in wood, thereby maintaining its anti-corrosion effect in a humid environment for a long time. The cross-linked structure formed by polyborates is more complex and stable, which significantly improves the anti-corrosion performance and durability. Although sodium fluoborate has certain anti-corrosion properties, due to its high solubility and the presence of fluorine, its loss rate is high under wet conditions, and its anti-corrosion effect is not as good as sodium tetraborate. Sodium metaborate has the weakest stability and anti-corrosion effect due to its lowest boron content and high solubility. Therefore, the anti-corrosion performance is ranked as Example 6 (sodium tetraborate) > Example 4 (sodium fluoborate) > Example 5 (sodium metaborate).
[0091] Compared with Example 6, Example 7 has a better anticorrosion effect. The main reason is that the tridecyl borate used has higher hydrophobicity and anti-loss performance compared with sodium tetraborate. Sodium tetraborate is a hydrophilic compound that is easily soluble in water during wood anticorrosion treatment, and the boron compound formed is easily dissolved and lost in a humid environment, thereby reducing the anticorrosion effect. However, tridecyl borate shows strong hydrophobicity and is insoluble in water due to its long-chain alkyl structure. When using tridecyl borate to treat wood, the compound can form a hydrophobic protective layer on the surface and inside of the wood, effectively preventing moisture from entering the wood, improving the waterproof performance of the wood, and reducing the loss of preservatives. In addition, the boron element provided by tridecyl borate reacts with polyhydroxy compounds (such as cellulose) in the wood to generate stable boron compounds, while its long-chain alkyl structure forms a hydrophobic barrier on the surface of the wood, further enhancing the durability of the anticorrosion effect.
[0092] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that are not conceived through creative work should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined in the claims.
Claims
1. A method for preparing a corrosion-resistant oak board, comprising soaking the oak board in a wood preservative liquid, characterized in that: The wood preservative liquid comprises dodecyldimethylbenzyl ammonium chloride and a boron-containing compound.
2. The method for preparing the corrosion-resistant oak board according to claim 1, characterized in that: The wood preservative liquid comprises the following raw materials in percentage by weight: 1-5 wt % of dodecyl dimethyl benzyl ammonium chloride and 1-4 wt % of a boron-containing compound.
3. The method for preparing the corrosion-resistant oak board according to claim 1, characterized in that: The boron-containing compound is at least one of sodium fluoroborate, sodium metaborate and sodium tetraborate.
4. The method for preparing the corrosion-resistant oak board according to claim 1, characterized in that: The wood preservative solution further comprises hexamethylene diisocyanate and trimethoxy (3,3,3-trifluoropropyl) silane.
5. The method for preparing the corrosion-resistant oak board according to claim 4, characterized in that: The wood preservative liquid comprises the following raw materials in percentage by weight: 2-4 wt % of dodecyldimethylbenzyl ammonium chloride, 2-3 wt % of a boron-containing compound, 0.2-0.8 wt % of hexamethylene diisocyanate and 0.2-0.8 wt % of trimethoxy (3,3,3-trifluoropropyl) silane.
6. The method for preparing the corrosion-resistant oak board according to claim 5, characterized in that: The wood preservative liquid comprises the following raw materials in percentage by weight: 2-4wt% of dodecyldimethylbenzyl ammonium chloride, 2-3wt% of boron-containing compounds, 0.2-0.8wt% of hexamethylene diisocyanate, 0.2-0.8wt% of trimethoxy (3,3,3-trifluoropropyl) silane, 0.5-1.5wt% of surfactant, 3-7wt% of ethanol, and the balance is water.
7. The method for preparing the corrosion-resistant oak board according to any one of claims 1 to 6, characterized in that: The soaking step is a vacuum pressure soaking process.
8. The method for preparing the corrosion-resistant oak board according to claim 7, characterized in that: The vacuum pressure soaking process has a vacuum degree of 0.1-0.6Mpa and a soaking time of 60-120 minutes.
9. The method for preparing the corrosion-resistant oak board according to claim 8, characterized in that: The vacuum pressure soaking process is a two-stage vacuum pressure soaking process, wherein the first stage of the vacuum pressure soaking process has a vacuum degree of 0.1-0.3Mpa and a soaking time of 30-60 minutes; the second stage of the vacuum pressure soaking process has a vacuum degree of 0.4-0.6Mpa and a soaking time of 30-60 minutes.
10. A corrosion-resistant oak board, characterized in that: The method is prepared by any one of claims 1 to 9.
Citation Information
Patent Citations
Wood antiseptic treatment method and antiseptic wood prepared using the said method
CN101422913A
Wood preservative and method for wood preservation
CN102066062A
Production method of high-temperature heating modified rubber wood floor
CN103072165A
Anticorrosive antibacterial wood production method
CN104858956A
Wood anticorrosion protective agent
CN104858967A