Forming process of polyimide profile
By adding carbon fiber powder and pre-pressing to the polyimide profile molding process, combined with heat treatment and stress relief treatment, the problem of low molding rate of thermosetting polyimide sheets is solved, the molding characteristics and qualification rate are improved, and the high thickness is satisfied. Forming needs of sheet metal.
Patent Information
- Application Number
- CN202410565746.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2024-10-01
AI Technical Summary
There is a problem of low molding rate during the molding process of thermosetting polyimide sheets. Especially for sheets with thickness greater than 35mm, the pass rate is low, and the molding process requires high equipment.
A polyimide profile molding process is used, including mixing, heat treatment and hot press molding. Polyimide powder and carbon fiber powder are mixed by heating in a mixer, pre-pressed and stress relieved, and a release agent is used. And control the molding temperature and pressure to ensure uniform mixing and stability of polyimide powder.
It improves the molding characteristics and qualification rate of polyimide sheets, ensures the mechanical and thermal properties of polyimide profiles, and reduces equipment requirements and stress changes during the molding process.
Smart Images

Figure CN118721476A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyimide resin molding, in particular to a molding process of a polyimide profile. Background Art
[0002] Due to its excellent temperature resistance and mechanical properties, imide resins are widely used in demanding electrical insulation, heat insulation and wear resistance fields such as aerospace components, semiconductor processing, automobile manufacturing and energy production. Depending on the structure of polyimide, its temperature resistance also varies. Among them, fully aromatic polyimide has become a research hotspot in recent years due to its excellent high temperature resistance. Since the molecular structure of thermosetting polyimide contains repeated aromatic rings and imide groups, the material has excellent mechanical properties, thermal properties, flame retardant properties, dielectric properties, environmental properties, etc. However, although thermosetting polyimide materials have the above-mentioned excellent comprehensive properties, their poor processing performance and difficulty in molding have greatly limited their application areas; especially in the mechanical and electronic fields, there is more demand for high-thickness PI sheets, but the current product qualification rate of thermosetting polyimide sheets with a thickness of more than 35mm is even less than 50%. The molding process of thermosetting polyimide sheets is a process in which its molecular chains produce gelation and orientation, which requires high molding temperature (greater than 400°C) and high molding pressure (greater than 100MPa), so the requirements for equipment are very high. In view of the particularity of the polyimide material itself and the existing molding molds, it is necessary to make corresponding adjustments to the process to improve the qualified rate of polyimide sheet molding. Therefore, a molding process for polyimide profiles is needed. Summary of the invention
[0003] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a molding process of a polyimide profile, so as to solve the problem of low molding rate of polyimide sheets in the prior art.
[0004] To achieve the above objectives and other related objectives, the present invention provides the following technical solutions:
[0005] A forming process of a polyimide profile comprises: mixing: taking 30-40 parts of polyimide powder and 10-15 parts of ground carbon fiber powder, adding the mixed materials into a mixer, and heating the inside of the mixer, the heating temperature is controlled at 90-150° C., and the stirring time is 7-9 minutes;
[0006] Heat treatment: putting the mixed polyimide powder into an oven for heat treatment at a heating temperature of 150 to 270° C. for 2 hours;
[0007] Hot pressing molding: open the mold, apply a release agent in the mold cavity, put the heated polyimide powder into the mold cavity, and pressurize and vulcanize the mold at the same time. The molding temperature is 350°C, the molding pressure is 15MPA, and the holding time is 4 hours;
[0008] Cool and take out after cooling naturally.
[0009] To implement the above technical solution, by adding ground carbon fiber powder and mixing it with polyimide powder in a blender, a mixed polyimide synthetic powder can be obtained. Compared with pure polyimide powder, the mixed polyimide powder has better molding properties. By heating inside the blender, the heating temperature is controlled at 90 to 150°C, and the stirring time is 7 to 9 minutes, the mixing effect of the carbon fiber powder and the polyimide powder can be improved.
[0010] By placing the mixed polyimide powder into an oven for heat treatment at a heating temperature of 150 to 270° C. for 2 hours, the carbon fiber powder and the polyimide powder can be fully mixed and more evenly mixed, thereby improving the degree of mixing of the two.
[0011] Hot pressing molding, open the mold, apply a release agent in the mold cavity, put the heated polyimide powder into the mold cavity, and pressurize and vulcanize the mold at the same time. The molding temperature is 350°C, the molding pressure is 15MPA, and the holding time is 4 hours. Maintaining a fixed pressure and controlling the pressing time can ensure the molding effect of the polyimide powder.
[0012] In one embodiment of the present invention, the mixed polyimide powder is pre-pressed before hot pressing. During the pre-pressing, the polyimide powder is first placed in a dedicated mold cavity and pre-pressed to give the polyimide powder an initial shape.
[0013] To implement the above technical solution, the mixed polyimide powder is pre-pressed before hot pressing, so that the polyimide powder can be pre-formed to facilitate subsequent hot pressing. The pre-pressing can also ensure the stability of the polyimide powder and will not cause too much change during subsequent hot pressing.
[0014] In one embodiment of the present invention, during the pre-pressing process, the temperature of the mold is controlled in two steps. First, the mold temperature is raised to 300°C, and a pressing is performed with the pressure controlled at 10 MPA for 30 minutes. Then, the mold temperature is raised to 330°C, and a second pressing is performed with the pressure controlled at 12 MPA for 30 minutes. After two pre-pressings, the polyimide powder can form an initial form.
[0015] By implementing the above technical solution and dividing the pre-pressing process into primary pressing and secondary pressing, the molding effect of the polyimide powder can be improved without damaging the polyimide powder, thereby improving the molding effect of subsequent hot pressing.
[0016] In one embodiment of the present invention, the polyimide profile after hot pressing is also subjected to stress relief treatment. The demolded polyimide sheet is placed in an oven for heat treatment and kept warm for 2 hours. The temperature in the oven is controlled at an initial temperature of 330°C and gradually decreases over time, decreasing by 90°C after 2 hours.
[0017] To implement the above technical solution, the demolded polyimide sheet is placed in an oven for heat treatment, which can avoid deformation of the polyimide profile after hot pressing, reduce the stress change after hot pressing treatment, and ensure that the hot pressing product will not be excessively deformed during the cooling process.
[0018] In one embodiment of the present invention, during mixing, the speed of the mixer is controlled at 150 RPM for 10 minutes, and then the speed is increased to 300 RPM and stirred for 30 minutes to mix the polyimide powder.
[0019] To implement the above technical solution, in order to better mix the polyimide powder without crushing the fiber powder and ensure the mixing effect, stir at a low speed for a period of time. After the fiber powder and the polyimide powder are fully in contact, increase the stirring speed so that the two can be fully mixed.
[0020] In one embodiment of the present invention, after the stirring speed in the stirrer is controlled at 150 RPM for 10 minutes, 5 to 7 parts of an auxiliary agent are added, and the auxiliary agent includes carbon nanotubes.
[0021] To implement the above technical solution, the provision of the auxiliary agent can improve the full combination of the fiber powder and the polyimide powder, and can reduce the damage to the fiber powder and the polyimide powder during the stirring process.
[0022] In one embodiment of the present invention, during the hot pressing forming, the heating treatment of the mold includes heating the mold cavity and the upper pressing plate at the same time.
[0023] The above technical solution is implemented to ensure the molding effect of polyimide powder.
[0024] In one embodiment of the present invention, the release agent is silicone grease or talcum powder.
[0025] The above technical solution is implemented to facilitate the separation of the polyimide profile after subsequent molding.
[0026] In one embodiment of the present invention, during hot pressing molding, the thickness of the pressing material is calculated according to the pressing needs to determine the pressing depth in the mold cavity, and the pressing depth of the mold cavity pressure plate is adjusted to stop the pressing action after reaching the expected pressing depth to maintain the molding state.
[0027] The above technical solution is implemented, and the pre-calculated die depth is utilized to ensure the subsequent forming effect.
[0028] As described above, a molding process of a polyimide profile of the present invention has the following beneficial effects: by adding ground carbon fiber powder and mixing it with polyimide powder in a blender, a mixed polyimide synthetic powder can be obtained, which has better molding properties than pure polyimide powder. By heating inside the blender, the heating temperature is controlled at 90 to 150°C, and the stirring time is 7 to 9 minutes, the mixing effect of the carbon fiber powder and the polyimide powder can be improved.
[0029] By placing the mixed polyimide powder into an oven for heat treatment at a heating temperature of 150 to 270° C. for 2 hours, the carbon fiber powder and the polyimide powder can be fully mixed and more evenly mixed, thereby improving the degree of mixing of the two. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 Shown is a process flow chart of the molding process of the polyimide profile disclosed in the embodiment of the present invention. DETAILED DESCRIPTION
[0030] The following specific embodiments illustrate the implementation of the present invention, and those familiar with the technology can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.
[0031] The present invention provides a molding process of a polyimide profile, comprising: mixing: taking 30 to 40 parts of polyimide powder and 10 to 15 parts of ground carbon fiber powder, adding the mixed materials into a mixer, and heating the inside of the mixer, wherein the heating temperature is controlled at 90 to 150° C., and the stirring time is 7 to 9 minutes;
[0032] Heat treatment: putting the mixed polyimide powder into an oven for heat treatment at a heating temperature of 150 to 270° C. for 2 hours;
[0033] Hot pressing molding: open the mold, apply a release agent in the mold cavity, put the heated polyimide powder into the mold cavity, and pressurize and vulcanize the mold at the same time. The molding temperature is 350°C, the molding pressure is 15MPA, and the holding time is 4 hours;
[0034] Cool and take out after cooling naturally.
[0035] By adding ground carbon fiber powder and mixing it with polyimide powder in a blender, a mixed polyimide synthetic powder can be obtained. Compared with pure polyimide powder, the mixed polyimide powder has better molding properties. By heating inside the blender, the heating temperature is controlled at 90 to 150° C., and the stirring time is 7 to 9 minutes, the mixing effect of the carbon fiber powder and the polyimide powder can be improved.
[0036] By placing the mixed polyimide powder into an oven for heat treatment at a heating temperature of 150 to 270° C. for 2 hours, the carbon fiber powder and the polyimide powder can be fully mixed and more evenly mixed, thereby improving the degree of mixing of the two.
[0037] Hot pressing molding, open the mold, apply a release agent in the mold cavity, put the heated polyimide powder into the mold cavity, and pressurize and vulcanize the mold at the same time. The molding temperature is 350°C, the molding pressure is 15MPA, and the holding time is 4 hours. Maintaining a fixed pressure and controlling the pressing time can ensure the molding effect of the polyimide powder.
[0038] The mixed polyimide powder must be pre-pressed before hot pressing. During the pre-pressing, the polyimide powder is first placed in a dedicated mold cavity and pre-pressed to give the polyimide powder an initial shape.
[0039] By pre-pressing the mixed polyimide powder before hot pressing, the polyimide powder can be pre-formed, which is convenient for subsequent hot pressing. Pre-pressing can also ensure the stability of the polyimide powder and will not cause too much change during subsequent hot pressing.
[0040] During the pre-pressing process, the temperature control of the mold is divided into two steps. First, the mold temperature is raised to 300°C, and a pressing is performed with the pressure controlled at 10MPA for 30 minutes. Then, the mold temperature is raised to 330°C, and a second pressing is performed with the pressure controlled at 12MPA for 30 minutes. After two pre-pressings, the polyimide powder can form an initial shape.
[0041] Dividing the pre-pressing process into primary pressing and secondary pressing can improve the molding effect of the polyimide powder without causing damage to the polyimide powder, thereby improving the molding effect of subsequent hot pressing molding.
[0042] The polyimide profile after hot pressing will also undergo stress relief treatment. The demoulded polyimide sheet is placed in an oven for heat treatment and kept warm for 2 hours. The temperature in the oven is controlled at an initial temperature of 330°C and gradually decreases over time, decreasing by 90°C after 2 hours.
[0043] Placing the demoulded polyimide sheet into an oven for heat treatment can avoid deformation of the polyimide profile after hot pressing, reduce stress changes after hot pressing treatment, and ensure that the hot pressing product will not be excessively deformed during the cooling process.
[0044] During mixing, the speed of the mixer was controlled at 150 RPM for 10 minutes, and then the speed was increased to 300 RPM and stirred for 30 minutes to mix the polyimide powder.
[0045] In order to better mix the polyimide powder without crushing the fiber powder and ensure the mixing effect, stir at a low speed for a period of time. After the fiber powder and the polyimide powder are fully in contact, increase the stirring speed so that the two can be fully mixed.
[0046] After stirring for 10 minutes at a speed of 150RPM in the mixer, 5 to 7 parts of an auxiliary agent are added, wherein the auxiliary agent includes carbon nanotubes. The setting of the auxiliary agent can improve the full combination of the fiber powder and the polyimide powder, and can reduce the damage to the fiber powder and the polyimide powder during the stirring process.
[0047] During hot pressing, the heating treatment of the mold includes heating the mold cavity and the upper pressing plate at the same time to ensure the molding effect of the polyimide powder. The release agent is silicone grease or talcum powder to facilitate the removal of the polyimide profile after subsequent molding.
[0048] During hot pressing, the thickness of the pressing material is calculated according to the pressing needs to determine the pressing depth in the mold cavity. After the pressing depth of the mold cavity pressing plate is adjusted to reach the expected pressing depth, the pressing action is stopped and the molding state is maintained. The pre-calculated pressing depth is used to ensure the subsequent molding effect.
[0049] The present invention adds ground carbon fiber powder and mixes it with polyimide powder in a blender to obtain a mixed polyimide synthetic powder. Compared with pure polyimide powder, the mixed polyimide synthetic powder has better molding properties. By heating inside the blender, the heating temperature is controlled at 90 to 150° C. and the stirring time is 7 to 9 minutes, the mixing effect of the carbon fiber powder and the polyimide powder can be improved.
[0050] By placing the mixed polyimide powder into an oven for heat treatment at a heating temperature of 150 to 270° C. for 2 hours, the carbon fiber powder and the polyimide powder can be fully mixed and more evenly mixed, thereby improving the degree of mixing of the two.
[0051] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. All equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A molding process for a polyimide profile, characterized in that: include: Mixing: Take 30-40 parts of polyimide powder and 10-15 parts of ground carbon fiber powder, mix them and add them into a blender, and heat the inside of the blender at a temperature of 90-150°C and stir for 7-9 minutes; Heat treatment: putting the mixed polyimide powder into an oven for heat treatment at a heating temperature of 150 to 270° C. for 2 hours; Hot pressing molding: open the mold, apply a release agent in the mold cavity, put the heated polyimide powder into the mold cavity, and pressurize and vulcanize the mold at the same time. The molding temperature is 350°C, the molding pressure is 15MPA, and the holding time is 4 hours; Cool and take out after cooling naturally.
2. The molding process of the polyimide profile according to claim 1, characterized in that: The mixed polyimide powder must be pre-pressed before hot pressing. During the pre-pressing, the polyimide powder is first placed in a dedicated mold cavity and pre-pressed to give the polyimide powder an initial shape.
3. The molding process of the polyimide profile according to claim 1, characterized in that: During the pre-pressing process, the temperature of the mold is controlled in two steps. First, the mold temperature is raised to 300°C, and a pressing is performed with the pressure controlled at 10 MPA for 30 minutes. Then, the mold temperature is raised to 330°C, and a second pressing is performed with the pressure controlled at 12 MPA for 30 minutes. After two pre-pressings, the polyimide powder can form an initial form.
4. The molding process of the polyimide profile according to claim 1, characterized in that: The polyimide profile after hot pressing will also undergo stress relief treatment. The demoulded polyimide sheet is placed in an oven for heat treatment and kept warm for 2 hours. The temperature in the oven is controlled at an initial temperature of 330°C and gradually decreases over time, decreasing by 90°C after 2 hours.
5. The molding process of the polyimide profile according to claim 1, characterized in that: During mixing, the speed of the mixer was controlled at 150 RPM for 10 minutes, and then the speed was increased to 300 RPM and stirred for 30 minutes to mix the polyimide powder.
6. The molding process of the polyimide profile according to claim 1, characterized in that: The speed of the stirrer is controlled at 150 RPM and stirred for 10 minutes, and then 5 to 7 parts of an auxiliary agent are added, wherein the auxiliary agent includes carbon nanotubes.
7. The molding process of the polyimide profile according to claim 1, characterized in that: During the hot pressing molding, the heating treatment of the mold includes heating the mold cavity and the upper pressing plate at the same time.
8. The molding process of the polyimide profile according to claim 1, characterized in that: The release agent is silicone grease or talcum powder.
9. The molding process of the polyimide profile according to claim 1, characterized in that: During hot pressing, the thickness of the pressing material is calculated according to the pressing needs to determine the pressing depth in the mold cavity. After the pressing depth of the mold cavity pressing plate is adjusted to reach the expected pressing depth, the pressing action is stopped to maintain the molding state.
Citation Information
Patent Citations
Microwave forming method for thermoset polyimide panels
CN107139371A
Molding process of polyimide profile
CN107718388A
Polyimide resin molding process
CN110181735A
Preparation method of high-permeability soft magnetic material
CN115662767A
Beryllium copper wire for high-voltage switch contact finger spring and production process of beryllium copper wire