Rubber-metal laminate and gasket

By increasing the modulus value and content of the rubber layer in the rubber-metal laminate, combined with a high content of carbon black and a specific adhesive, the problem of rubber layer overflow is solved and excellent sealing is achieved.

CN118721887APending Publication Date: 2024-10-01NOK CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410846596.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-03-17
Filing Date
2021-02-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing rubber-metal laminate easily causes the rubber layer to overflow when compressive stress is applied, and the sealing performance is insufficient. The existing improvement measures such as filling materials and cross-linking agents have limited effect.

Method used

The 100% modulus value of the rubber layer is more than 8.5MPa, the thickness is more than 80μm, and the rubber layer contains more than 30% carbon black, using phenolic resin and epoxy resin as adhesives, through free phenolic resin and ring The combination of oxy-resin is bonded to form a rubber-metal laminate with moderate elastic modulus.

Benefits of technology

It effectively prevents the rubber layer from overflowing under compressive stress, improves the sealing performance of the sealing object components, avoids sealing deterioration, and maintains the softness of the rubber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004915854560000171
    Figure BDA0004915854560000171
Patent Text Reader

Abstract

The present invention relates to a rubber-metal laminate and a gasket, the rubber-metal laminate comprising a metal member and a rubber layer provided on the metal member, the rubber layer having a 100% modulus value according to JIS K6251 of 8.5 MPa or more and a thickness of 80 [mu] m or more and 200 [mu] m or less, and the amount of the rubber layer being less than 100 parts by mass per 100 parts by mass of the rubber component. The rubber layer contains from 85 parts by mass to 250 parts by mass (inclusive) of carbon black. According to the present invention, it is possible to realize a rubber-metal laminate and a gasket which are capable of preventing overflow of a rubber layer when compressive stress is applied, and which have excellent sealing properties of a member to be sealed.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a patent application with application number 202180022003.3 (international application number PCT / JP2021 / 006898), application date February 24, 2021, and invention name “Rubber-metal laminate and gasket”. Technical Field

[0002] The present invention relates to a rubber metal laminate and a gasket. Background Art

[0003] In the past, a metal gasket has been proposed for sealing between two components such as a cylinder head and a cylinder block of an internal combustion engine (for example, see Patent Document 1). The metal gasket includes a rubber metal laminate including a metal substrate and rubber layers provided on both main surfaces of the metal substrate. In the metal gasket described in Patent Document 1, the rubber metal laminate is fastened between the cylinder head and the cylinder block to seal the portion between the cylinder head and the cylinder block, which is a sealing target component.

[0004] However, in the metal gasket described in Patent Document 1, since the rubber metal laminate is fastened between metal members such as a cylinder head and a cylinder block, a strong compressive stress is applied to the rubber metal laminate during use. In such a rubber metal laminate, there is a case where the rubber layer is deformed due to the compressive stress applied during use, and the rubber overflows from the rubber metal laminate, and the desired function cannot be obtained.

[0005] In order to improve the overflow of rubber caused by the deformation of the rubber layer, it is effective to add fillers such as carbon black and silica to the rubber layer to increase the hardness of the rubber layer. However, there are cases where the sealing of the sealing object component generated by the rubber layer decreases when the hardness of the rubber layer increases. In addition, in order to improve the overflow of rubber, studies have been conducted to increase the crosslinking density of the rubber layer by increasing the amount of sulfur used as a crosslinking agent in the rubber layer composition, but even if the crosslinking density of the rubber layer is increased, it is not expected that there will be a significant improvement in the overflow of the rubber. In this way, in existing rubber-metal laminates, the actual situation is that only increasing the hardness sometimes cannot fully improve the overflow of the rubber, and the relationship between the physical properties of the rubber and the overflow has not been found.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2003-130224 Summary of the invention

[0009] Technical problem to be solved by the invention

[0010] The present invention has been made in view of such actual circumstances, and provides a rubber-metal laminate and a gasket which can prevent the rubber layer from leaking out when compressive stress is applied and have excellent sealing properties for a sealed member.

[0011] Technical means for solving technical problems

[0012] A rubber-metal laminate according to an embodiment of the present invention includes a metal member and a rubber layer provided on the metal member, wherein the rubber layer has a 100% modulus value of 8.5 MPa or more based on JIS K6251 and a thickness of 80 μm or more.

[0013] In one embodiment of the present invention, the rubber layer has a 100% modulus value based on JIS K6251 of 10.5 MPa or more.

[0014] In one embodiment of the present invention, the rubber layer has an elongation value of 100% or more in accordance with JIS K6251.

[0015] In one embodiment of the present invention, the thickness of the rubber layer is 200 μm or less.

[0016] In one embodiment of the present invention, the rubber layer contains 30% by mass or more of carbon black based on the total mass of the rubber layer.

[0017] In one embodiment of the present invention, the metal member and the rubber layer are bonded to each other by at least one adhesive selected from the group consisting of phenolic resins and epoxy resins.

[0018] In one embodiment of the present invention, the rubber layer contains nitrile rubber.

[0019] A gasket according to an embodiment of the present invention includes the rubber metal laminate described above.

[0020] Effects of the Invention

[0021] According to the present invention, it is possible to realize a rubber-metal laminate and a gasket which can prevent the rubber layer from leaking out when compressive stress is applied and have excellent sealing properties for a sealed member. DETAILED DESCRIPTION

[0022] Hereinafter, an embodiment of the present invention will be described in detail. The rubber metal laminate of an embodiment of the present invention is suitable for use as a sealing component such as a gasket. The rubber metal laminate of this embodiment includes a metal component and a rubber layer, which is provided on the main surface of at least one side of the metal component. The 100% modulus value of the rubber layer is 8.5 MPa or more and the thickness of the rubber layer is 80 μm or more. Since the 100% modulus value of the rubber layer is 8.5 MPa or more and the thickness is 80 μm or more, the elastic modulus of the rubber layer is moderately improved. As a result, compared with the case where the hardness of the rubber layer is increased by a filling material, the rubber metal laminate can prevent the deterioration of the sealing performance and can ensure the elastic modulus required for the rubber layer. As a result, even when compressive stress is applied to the rubber metal laminate, the rubber layer can be further prevented from overflowing from the rubber metal laminate, and a rubber metal laminate with excellent sealing performance of the sealed object component can be realized. Hereinafter, various structural elements of the rubber metal laminate of this embodiment will be described in detail.

[0023] (Metal components)

[0024] As metal components, for example, metal plates such as iron, stainless steel, aluminum, magnesium, galvanized steel, and copper can be used. As iron, for example, cold rolled steel plates (SPCC: Steel Plate Cold Commercial), high-tensile steel plates, and mild steel plates can be used. In addition, as stainless steel, for example, ferritic, martensitic, austenitic, and other stainless steel plates can be used. Specific examples of stainless steel include, for example, SUS304, SUS301, SUS301H, and SUS430. As aluminum, aluminum plates and aluminum die-cast plates can be used.

[0025] The metal parts are preferably used in a state where the surface is degreased by alkali degreasing treatment, etc. In addition, the metal parts can be used after roughening the metal surface by shot blasting, Scotch-Brite (registered trademark), hair line treatment, dull finish, etc. as needed.

[0026] For metal components, it is preferred that the bonding surface with the adhesive is subjected to a substrate treatment (surface treatment). As the substrate treatment, there is no particular limitation, and known substrate treatments can be used. As the substrate treatment, when using iron materials and stainless steel materials such as cold-rolled steel sheets and high-tensile steel sheets as metal components, it is preferred to use various chemical conversion treatment methods, electroplating using metals such as zinc, hot-dip plating and other plating methods. As chemical conversion treatment agents for metal components, for example, phosphoric acid treatment agents such as zinc phosphate treatment agents and iron phosphate treatment agents, coating-type chromate treatment agents, etc. can be cited. As chemical conversion treatment agents, from the viewpoint of environmental protection, chromium-free chemical conversion treatment agents that are substantially free of chromium are preferred.

[0027] The base treatment of metal parts using a chemical conversion treatment agent is carried out by contacting the chemical conversion treatment agent with the metal parts using a known contact method such as spraying, dipping, brushing, and roller coating. In the case of a reactive chemical conversion treatment agent, it is required to ensure the time and temperature required for the reaction.

[0028] The thickness of the metal component is appropriately set according to the purpose of the rubber metal laminate. When the rubber metal laminate is used for sealing parts such as gaskets, the thickness of the metal component is preferably 100 μm or more and 2000 μm or less, more preferably 200 μm or more and 1000 μm or less, and further preferably 300 μm or more and 500 μm or less.

[0029] The rubber-metal laminate preferably forms a primer coating on the metal component in addition to the base treatment, or forms a primer coating on the metal component instead of the base treatment. By performing the base treatment or providing the primer coating, the adhesion between the rubber layer and the metal component in the rubber-metal laminate can be improved, and the heat resistance and water resistance of the rubber-metal laminate can be greatly improved. In addition, the rubber-metal laminate can be suitably used as a laminated composite metal, i.e., a gasket, by performing the base treatment or forming the primer coating, which is formed by laminating the rubber-metal laminate with other metal plates.

[0030] The primer coating can be provided by inorganic compounds such as compounds of metals such as silicon compounds, titanium, zirconium, vanadium, aluminum, molybdenum, tungsten, manganese, zinc and cerium, and their oxides, organic compounds such as silicone resins, phenolic resins, epoxy resins and polyurethanes, etc. The primer coating can be provided by using a primer solution generally available on the market, or by using primer solutions based on various known technologies.

[0031] The primer coating is provided by a primer solution, which is a solution obtained by dissolving or dispersing raw materials including the above-mentioned various inorganic compounds and organic compounds in an organic solvent or an aqueous solvent. As the usable organic solvent, for example, alcohols such as methanol, ethanol and isopropanol, ketones such as acetone and methyl ethyl ketone, etc. can be cited. The primer solution can also be prepared as an aqueous solution using an aqueous solvent as long as the liquid stability can be maintained.

[0032] The obtained primer solution is applied to the metal member by spraying, dipping, brushing, rolling, etc. The primer coating is provided by drying the primer solution applied to the metal member at room temperature or with hot air, or by performing a sintering treatment.

[0033] (Adhesive)

[0034] The adhesive bonds the rubber layer to the metal member. As the adhesive, a commercially available adhesive such as a phenolic resin, an epoxy resin, a polyurethane resin, and a silane is used. These adhesives can be appropriately selected according to the application of the rubber-metal laminate.

[0035] In the rubber-metal laminate, the metal component and the rubber layer are preferably bonded by at least one adhesive selected from the group consisting of phenolic resins and epoxy resins. As a result, the rubber-metal laminate improves the adhesion between the metal component and the rubber layer, thereby further preventing the rubber layer from overflowing from the rubber-metal laminate when compressive stress is applied, and further improving the sealing performance of the sealed object component.

[0036] As the phenolic resin, for example, novolac phenolic resin and resol phenolic resin can be used. Novolac phenolic resin and resol phenolic resin can be used alone or in combination of two or more. In addition, as the adhesive, an adhesive containing novolac phenolic resin and resol phenolic resin and unvulcanized nitrile rubber can also be used.

[0037] As the novolac type phenolic resin, a product obtained by condensing phenols and formaldehyde in the presence of an acid catalyst can be used. As phenols, for example, phenol, p-cresol, m-cresol, p-tert-butylphenol, p-phenylphenol, bisphenol A and the like having 2 or 3 replaceable hydrogen atoms at at least one of the ortho and para positions relative to the phenolic hydroxyl group can be used. These phenolic resins can be used alone or in combination of two or more. As the acid catalyst, for example, oxalic acid, hydrochloric acid and maleic acid can be used. Among them, as the novolac type phenolic resin, from the viewpoint of improving the adhesion between the metal component and the rubber layer, it is preferred to have a melting point of more than 80°C and less than 150°C, and it is more preferred to use m-cresol and formaldehyde to obtain the novolac type phenolic resin, and have a melting point of more than 120°C.

[0038] As the resol type phenolic resin, the product obtained by condensing phenols and formaldehyde in the presence of an alkali catalyst can be used. As phenols, for example, phenol, p-cresol, m-cresol, and p-tert-butylphenol, p-phenylphenol, bisphenol A and the like having 2 or 3 replaceable hydrogen atoms in at least one of the ortho and para positions relative to the phenolic hydroxyl group can be used. These phenolic resins can be used alone or in combination of two or more. As the alkali catalyst, for example, alkali metal hydroxides such as ammonia and sodium hydroxide, magnesium hydroxide, sodium carbonate and the like can be used.

[0039] As epoxy resin, bisphenol A type, cresol novolac type, biphenyl type, brominated epoxy resin etc. can be cited. These epoxy resins can be used alone or in combination of two or more. Among these resins, from the viewpoint of being easy to obtain commercially available products and the viewpoint of excellent heat resistance, bisphenol A type epoxy resin and cresol novolac type epoxy resin are preferred. As bisphenol A type epoxy resin, for example, commercially available products such as trade names "EPICLON (registered trademark) 860", "EPICLON (registered trademark) 1055", "EPICLON (registered trademark) 2050", "EPICLON (registered trademark) 3050", "EPICLON (registered trademark) 4050", "EPICLON (registered trademark) 7050", "EPICLON (registered trademark) HM-091" made by DIC can be used. In addition, as commercial products of cresol novolac epoxy resin, for example, commercial products such as "EPICLON (registered trademark) N-660", "EPICLON (registered trademark) N-670", "EPICLON (registered trademark) N-680", and "EPICLON (registered trademark) N-690" manufactured by DIC Corporation can be used.

[0040] The above-mentioned various adhesives are used as solutions obtained by dissolving in organic solvents. As organic solvents, for example, ketones such as methyl ethyl ketone and methyl isobutyl ketone, aromatic hydrocarbons such as toluene and xylene, etc. can be used. These organic solvents can be used alone or in combination of two or more.

[0041] For the adhesive, for example, the resol type phenolic resin is preferably mixed in a ratio of 10 to 1000 parts by mass relative to 100 parts by mass of the novolac type phenolic resin, and more preferably in a ratio of 60 to 400 parts by mass. The adhesive can prevent the adhesiveness of the rubber layer from decreasing by making the resol type phenolic resin less than 1000 parts by mass relative to 100 parts by mass of the novolac type phenolic resin, and can prevent the adhesiveness to the surface of the metal component from decreasing by making the resol type phenolic resin more than 10 parts by mass.

[0042] From the viewpoint of improving the adhesion between the metal component and the rubber layer, the adhesive is preferably provided on the metal component formed with the primer coating. In addition, the adhesive layer may be provided as a single layer or multiple layers. The adhesive layer may also be provided as a multi-stage structure by further providing a phenolic adhesive layer on the adhesive layer after forming a phenolic adhesive layer containing an organic metal compound on the primer coating provided on the metal component. By providing the adhesive layer with such a multi-stage structure, the adhesion between the primer coating and the rubber layer can be made stronger.

[0043] The adhesive is prepared into an adhesive solution having a solid content concentration of 1 mass % or more and 10 mass % or less using ketone organic solvents such as acetone, methyl ethyl ketone and methyl isobutyl ketone and their mixed solvents. After the adhesive solution is applied to the metal component, it is dried and sintered for 1 minute or more and 30 minutes or less at a temperature of 100° C. or more and 250° C. or less to form an adhesive layer. The amount of adhesive applied is preferably 50 mg / m 2 Above and 2000mg / m 2 In addition, the adhesive is preferably applied so that the thickness of the adhesive layer after drying is 0.5 μm or more and 5 μm or less.

[0044] (Rubber layer)

[0045] In the rubber-metal laminate of the present embodiment, the 100% modulus value of the rubber layer according to JIS K6251 is 8.5 MPa or more. As a result, even when a high compressive stress is applied to the rubber-metal laminate, the rubber layer has an appropriate elastic modulus, and the overflow of the rubber layer from the rubber-metal laminate can be suppressed, thereby improving the sealing performance of the sealed object member. In addition, since the rubber-metal laminate has an appropriate elastic modulus without increasing the hardness of the rubber layer, the deterioration of the sealing performance is prevented, the softness of the rubber is maintained, and the sealing performance of the sealed object member is improved.

[0046] From the viewpoint of further improving the above-mentioned effect, the 100% modulus value of the rubber layer is more preferably 10.5 MPa or more, more preferably 12 MPa or more, and preferably 30 MPa or less, more preferably 25 MPa or less, and more preferably 20 MPa or less. By setting the 100% modulus value to 10.5 MPa or more, the rubber-metal laminate can prevent the deterioration of the sealing performance and can fully ensure the elastic modulus required for the rubber layer. As a result, even when the rubber-metal laminate is subjected to compressive stress, the rubber layer can be further prevented from overflowing from the rubber-metal laminate, thereby further improving the sealing performance of the sealed object member.

[0047] Furthermore, in the rubber-metal laminate of the present embodiment, the elongation value of the rubber layer according to JIS K6251 is preferably 100% or more. Thus, since the elongation value of the rubber layer is within an appropriate range, even when compressive stress acts on the rubber-metal laminate, it is possible to further prevent the rubber layer from overflowing from the rubber-metal laminate, and further improve the sealing performance of the sealed object member. In addition, from the viewpoint of further improving the above-mentioned effect, the elongation value of the rubber layer is more preferably 140% or more, more preferably 170% or more, and preferably 300% or less, more preferably 240% or less, and more preferably 200% or less.

[0048] In addition, in the rubber metal laminate of the present embodiment, from the viewpoint of obtaining an appropriate elastic modulus without excessively increasing the hardness of the rubber layer, preventing deterioration of the sealing performance and improving the sealing performance of the sealed object member, the hardness of the rubber layer based on JIS K6253 is preferably 60 to 100, more preferably 70 to 95, and even more preferably 80 to 90.

[0049] In addition, in the rubber metal laminate of the present embodiment, from the viewpoint of preventing the rubber layer from overflowing when compressive stress is applied and improving the sealing performance of the sealed object member, the tensile strength measured based on JIS K6251 is preferably 7.5 MPa to 30 MPa, more preferably 10 MPa to 27.5 MPa, and further preferably 12 MPa to 25 MPa.

[0050] For the rubber layer, various rubber materials can be used to obtain it within the scope of exerting the effect of the present invention. As the rubber material, for example, various rubber materials such as nitrile rubber (NBR: Nitrile Butadiene Rubber) as an acrylonitrile-butadiene copolymer, hydrogenated nitrile rubber (HNBR) in which the unsaturated bond of nitrile rubber is partially hydrogenated, and fluororubber can be cited. Among them, from the viewpoint of preventing the rubber layer from overflowing from the rubber metal laminate and improving the sealing performance, nitrile rubber and hydrogenated nitrile rubber are preferred, and nitrile rubber is more preferred. In addition, as a rubber layer, when used in various gaskets such as cylinder head gaskets for automobiles, it is preferred to include at least one rubber selected from the group consisting of fluororubber and nitrile rubber, preferably including nitrile rubber. By containing nitrile rubber in the rubber layer, the nitrile rubber contained in the rubber layer has appropriate elasticity, so even when compressive stress acts on the rubber metal laminate, it is possible to further prevent the rubber layer from overflowing from the rubber metal laminate, and further improve the sealing performance of the sealed object component. In addition, by crosslinking the rubber layer, more excellent heat resistance and adhesion can be obtained.

[0051] As the nitrile rubber, from the viewpoint of improving the adhesion between the rubber layer and the adhesive and improving the cold resistance, it is preferred that the bound acrylonitrile content is 18% or more and 48% or less, more preferably 31% or more and 42% or less, and in particular, medium-high nitrile with a bound acrylonitrile content of 31% or more and less than 36% is further preferred. In addition, as the nitrile rubber, from the viewpoint of improving the friction / wear resistance and improving the kneading processability, the Mooney viscosity ML 1+4( 100°C) is 30 or more and 85 or less, and the Mooney viscosity ML can be used 1+4( The acrylonitrile-butadiene copolymer rubber has a temperature (100° C.) of 40 to 70. As the nitrile rubber, a commercially available product such as “Nipol (registered trademark) DN3350” (manufactured by Nippon Zeon Co., Ltd.) can be used.

[0052] Furthermore, from the viewpoint of increasing the hardness of the rubber layer and preventing the rubber layer from protruding from the rubber metal laminate when compressive stress acts on the rubber metal laminate, the rubber layer is preferably formed using a rubber composition containing carbon black.

[0053] Examples of carbon black include hard carbon blacks such as super abrasion furnace (SAF) carbon black, intermediate super abrasion furnace (ISAF) carbon black, high abrasion furnace (HAF) carbon black, and easy processing channel (EPC) carbon black, and soft carbon blacks such as eXtra Conductive furnace (XCF) carbon black, fast extruding furnace (FEF) carbon black, general purpose furnace (GPF) carbon black, high stress furnace (HMF) carbon black, medium reinforcement furnace (SRF) carbon black, fine thermal decomposition furnace (FT) carbon black, and medium thermal decomposition furnace (MT) carbon black. These carbon blacks may be used alone or in combination of two or more. Among them, as carbon black, soft carbon black is preferred, and among soft carbon black, medium reinforcing carbon black and medium-grained thermal decomposition carbon black are more preferred. As carbon black, commercial products of medium-grained thermal decomposition carbon black such as "THERMAX (registered trademark) N990LSR" (manufactured by Cancarb) can be used, and commercial products of medium reinforcing carbon black such as "HTC#SS" (manufactured by Nippon Steel Carbon Co., Ltd.) and "ASAHI#50HG" (manufactured by Asahi Carbon Co., Ltd.) can also be used.

[0054] The amount of carbon black added is preferably 50 parts by mass or more and 500 parts by mass or less, more preferably 70 parts by mass or more and 350 parts by mass or less, and even more preferably 85 parts by mass or more and 250 parts by mass or less, relative to 100 parts by mass of the rubber component, from the viewpoint of preventing the rubber layer from protruding from the rubber metal laminate when compressive stress is applied to improve the sealing performance.

[0055] The amount of carbon black added is preferably 30% by mass or more and 80% by mass or less, more preferably 40% by mass or more and 70% by mass or less, and further preferably 50% by mass or more and 60% by mass or less, relative to the total mass of the rubber composition (rubber layer), from the viewpoint of preventing the rubber layer from overflowing from the rubber metal laminate when compressive stress is applied, so as to improve the sealing performance. By making the rubber layer contain 30% by mass or more of carbon black relative to the total mass of the rubber layer, the rubber metal laminate can prevent the deterioration of the sealing performance and ensure the elastic modulus required by the rubber layer. As a result, even when compressive stress acts on the rubber metal laminate, the rubber layer can be further prevented from overflowing from the rubber metal laminate, and the sealing performance of the sealed object component can be further improved.

[0056] Furthermore, when the carbon black is MT carbon black, the amount of the carbon black is preferably 50 parts by mass or more and 300 parts by mass or less, more preferably 70 parts by mass or more and 250 parts by mass or less, and even more preferably 85 parts by mass or more and 200 parts by mass or less, relative to 100 parts by mass of the rubber component, from the viewpoint of preventing the rubber layer from protruding from the rubber metal laminate when compressive stress is applied to improve the sealing performance.

[0057] When the carbon black is MT carbon black, the amount of the carbon black blended is preferably 45% by mass or more and 80% by mass or less, more preferably 50% by mass or more and 70% by mass or less, and even more preferably 55% by mass or more and 60% by mass or less, relative to the total mass of the rubber composition, from the viewpoint of preventing the rubber layer from protruding from the rubber metal laminate when compressive stress is applied to improve the sealing performance.

[0058] In addition, when the carbon black is SRF carbon black, from the viewpoint of preventing the rubber layer from overflowing from the rubber metal laminate when compressive stress is applied to improve the sealing performance, the amount of carbon black blended is preferably 45 parts by mass or more and 150 parts by mass or less, and more preferably 50 parts by mass or more and 125 parts by mass or less, relative to 100 parts by mass of the rubber component.

[0059] When the carbon black is SRF carbon black, the amount of carbon black blended is preferably 30% by mass or more and 70% by mass or less, more preferably 35% by mass or more and 65% by mass or less, and further preferably 40% by mass or more and 60% by mass or less, relative to the total mass of the rubber composition, from the viewpoint of preventing the rubber layer from protruding from the rubber metal laminate when compressive stress is applied to improve the sealing performance.

[0060] The rubber layer is provided by crosslinking the rubber composition after applying the rubber composition on the metal member or the primer coating. The rubber composition preferably contains a vulcanizing agent and a vulcanization accelerator. As the vulcanizing agent, for example, commercial products such as colloidal sulfur A (manufactured by Tsurumi Chemical Industry Co., Ltd.) and trade name "VULNOC (registered trademark) R" (4,4'-dithiodimorpholine: manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can be used. The amount of the vulcanizing agent is, for example, 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the rubber component.

[0061] As the vulcanization accelerator, various sulfur-containing vulcanization accelerators such as guanidine-based, aldehyde-amine-based, aldehyde-ammonia-based, thiazole-based, sulfenamide-based, thiourea-based, thiuram-based, dithiocarbamate-based and xanthate-based can be used. Among them, as the sulfur-containing vulcanization accelerator, tetramethylthiuram disulfide, tetrabenzylthiuram disulfide and N-cyclohexyl-2-benzothiazolylsulfenamide are preferred. In addition, as the vulcanization accelerator, commercial products such as trade names "NOCCELER (registered trademark) TBZTD" (tetrabenzylthiuram disulfide: manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), trade names "NOCCELER (registered trademark) CZ-P" (N-cyclohexyl-2-benzothiazolylsulfenamide: manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) and "NOCCELER (registered trademark) TT-P" (tetramethylthiuram disulfide: manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can be used. The amount of the vulcanization accelerator blended is, for example, 1 part by mass or more and 20 parts by mass or less relative to 100 parts by mass of the rubber component.

[0062] In addition, the rubber composition may also contain fillers such as calcium carbonate and silicon dioxide as needed. As calcium carbonate, various calcium carbonates such as heavy calcium carbonate and synthetic calcium carbonate can be used. In addition, as calcium carbonate, commercial products such as the trade name "WHITON SB-Red" (heavy calcium carbonate, manufactured by Beibei Powder Industry Co., Ltd.) can also be used. The blending amount of calcium carbonate is preferably 10 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the rubber component.

[0063] As silicon dioxide, various silicon dioxides can be used within the scope of the effect of the present invention. As silicon dioxide, for example, amorphous silicon dioxides such as the following dry silicon dioxide and wet silicon dioxide can be used, the dry silicon dioxide is manufactured by the thermal decomposition method of halogenated silicic acid or organosilicon compound, the silicon oxide (SiO) obtained by heating and reducing silica sand and gasifying is oxidized by air, etc., and the wet silicon dioxide is manufactured by the thermal decomposition method of sodium silicate, etc. In addition, as silicon dioxide, for example, commercial products such as trade name "Nipsil (registered trademark) E-74P" (Tosohsilica company system) can also be used. As the amount of silicon dioxide, it is preferably relative to 100 parts by mass of the rubber component, for example, more than 5 parts by mass and less than 50 parts by mass.

[0064] In addition, the rubber composition may contain plasticizers, acid acceptors such as zinc oxide, stearic acid, anti-aging agents, waxes and other additives commonly used in the rubber industry as needed. As plasticizers, for example, commercial products such as "ADKCIZER (registered trademark) RS107" (made by ADEKA) can be cited. The amount of the plasticizer is, for example, 1 part by mass or more and 50 parts by mass or less relative to 100 parts by mass of the rubber component.

[0065] As an acid acceptor, for example, commercial products such as zinc oxide (manufactured by Shodo Chemical Industry Co., Ltd.) can also be used. As stearic acid, for example, commercial products such as the trade name "DTST" (manufactured by Miyoshi Oil & Fats Co., Ltd.) can also be used. In addition, as an anti-aging agent, for example, commercial products such as the trade name "NOCRAC (registered trademark) 810-NA" (2,2,4-trimethyl-1,2-dihydroquinoline polymer: manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can also be used. In addition, as a wax, for example, commercial products such as the trade name "SUNTIGH (registered trademark) R" (microcrystalline wax: manufactured by Seiko Chemical Co., Ltd.) can also be used.

[0066] In addition, in the rubber-metal laminate of the present embodiment, the thickness of the rubber layer is 80 μm or more. Therefore, the relationship between the 100% modulus value and the thickness of the rubber layer is within an appropriate range, so that even when compressive stress acts on the rubber-metal laminate, the rubber layer can be further prevented from overflowing from the rubber-metal laminate, and the sealing performance of the sealed object member can be further improved.

[0067] The thickness of the rubber layer is preferably 200 μm or less, more preferably 90 μm or more and 150 μm or less, and even more preferably 100 μm or more and 140 μm or less from the viewpoint of further improving the above-mentioned effects. By making the thickness of the rubber layer 200 μm or less, the relationship between the 100% modulus value and the thickness of the rubber layer in the rubber-metal laminate is in an appropriate range, and the elastic modulus of the rubber layer is further improved. As a result, even when compressive stress acts on the rubber-metal laminate, the rubber layer can be further prevented from overflowing from the rubber-metal laminate, and the sealing performance of the sealed object component can be further improved.

[0068] <Method for producing rubber-metal laminate>

[0069] The rubber metal laminate of the above embodiment is manufactured using a metal component such as a stainless steel plate and the following rubber composition, which is a rubber component and carbon black, and a vulcanizer, a vulcanization accelerator, calcium carbonate, silica, a plasticizer and various additives as needed, and kneaded with a mixer such as a mixer, a kneader, a Banbury mixer or an open roller. The rubber metal laminate is manufactured in the following manner, that is, after applying the above rubber composition through an adhesive layer on a metal component that has been surface-treated as needed, for example, the rubber composition is vulcanized under the conditions of 160°C to 250°C and 0.5 minutes to 30 minutes to form a rubber layer, thereby manufacturing the rubber metal laminate. The rubber composition is preferably applied in a manner that the thickness of the rubber layer after coating is 50μm to 200μm. It should be noted that from the viewpoint of preventing the adhesion of rubber, the rubber metal laminate can also be coated with a coating agent such as a resin system and a graphite system on the rubber layer.

[0070] The method for applying the rubber composition to the metal member is not particularly limited as long as the rubber composition can be applied to the metal member. Examples of the method for applying the rubber composition include spraying, dipping, roller coating, and dispensing.

[0071] When manufacturing the rubber composition and when applying the rubber composition to the metal member, an organic solution may be added to the rubber composition as needed to adjust the viscosity. There is no particular limitation on the organic solvent, as long as the viscosity of the rubber composition can be adjusted to a desired viscosity. As the organic solvent, for example, methyl ethyl ketone, toluene and ethyl acetate may be cited. These organic solvents may be used alone or in combination of two or more.

[0072] As described above, according to the present embodiment, the 100% modulus value of the rubber layer is 8.5 MPa or more and the thickness is 80 μm or more, so the elastic modulus of the rubber layer is appropriately improved. As a result, the rubber-metal laminate can prevent the deterioration of the sealing performance compared to the case where the hardness of the rubber layer is increased by a filler, and can ensure the elastic modulus required for the rubber layer. As a result, even when compressive stress is applied to the rubber-metal laminate, the overflow of the rubber layer from the rubber-metal laminate can be further prevented, so that a rubber-metal laminate with excellent sealing performance of the sealed object member can be realized. In addition, in the rubber-metal laminate, the overflow performance has been improved by simply increasing the hardness of the rubber, but by focusing on the 100% modulus value for development, the overflow performance can be improved even with low hardness, and the improvement of the sealing performance can be expected. In addition, even if the rubber-metal laminate is not actually produced, the overflow performance of the rubber layer when the compressive stress is applied can be predicted by the 100% modulus value, which helps to reduce the evaluation process.

[0073] In addition, according to other embodiments, a gasket including the rubber metal laminate of the present embodiment can be obtained. According to the gasket of the present embodiment, since the 100% modulus value of the rubber layer is 8.5 MPa or more and the thickness is 80 μm or more, the elastic modulus of the rubber layer is moderately improved. As a result, the gasket can prevent the deterioration of the sealing performance and ensure the elastic modulus required for the rubber layer compared to the case where the hardness of the rubber layer is increased by a filling material. As a result, even when compressive stress is applied to the gasket, the rubber layer can be further prevented from overflowing from the gasket, so that a gasket with excellent sealing performance of the sealed object component can be realized.

[0074] Example

[0075] Hereinafter, the present invention will be described in more detail based on examples made to make the effects of the present invention clear. It should be noted that the present invention is not limited to the following examples in any way.

[0076] The inventors of the present invention produced the rubber-metal laminate of the above-mentioned embodiment, and conducted a compression test on the produced rubber-metal laminate to evaluate it. The contents of the investigation conducted by the inventors of the present invention will be described below.

[0077] (Example 1)

[0078] <Evaluation of the Thermoplasticity (TP) of Rubber>

[0079] 100 parts by mass of nitrile rubber (trade name "Nipol (registered trademark) DN3350", manufactured by Nippon Ozen Co., Ltd.), 151 parts by mass of carbon black A (medium thermal decomposition (MT: Mdeium Thermal) carbon black: trade name "THERMAX (registered trademark) N990LSR", manufactured by Cancarb Co., Ltd.), 5 parts by mass of zinc oxide (manufactured by Shodo Chemical Industry Co., Ltd.), 1 part by mass of stearic acid (trade name "DTST", manufactured by Miyoshi Oil & Fats Co., Ltd.), 2 parts by mass of an antioxidant (2,2,4-trimethyl-1,2-dihydroquinoline polymer: trade name "NOCRAC (registered trademark) 810-NA", manufactured by Ouchi Shinko Chemical Co., Ltd.), 2 parts by mass of microcrystalline wax (trade name "SUNTIGH (registered trademark) R", manufactured by Seiko Chemical Co., Ltd.), 2 parts by mass of a vulcanizing agent A (colloid Sulfur A (manufactured by Tsurumi Chemical Industry Co., Ltd.) 1.5 parts by mass, vulcanizing agent B (4,4'-dimorpholine disulfide: trade name "VULNOC (registered trademark) R", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) 1 part by mass, vulcanization accelerator A (tetrabenzylthiuram disulfide: trade name "NOCCELER (registered trademark) TBZTD", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) 5 parts by mass, and vulcanization accelerator B (N-cyclohexyl-2-benzothiazolylsulfenamide: trade name "NOCCELER (registered trademark) CZ-P", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) 4 parts by mass were kneaded with a kneader and an open roll to obtain a rubber composition. Next, the rubber composition was vulcanized by pressing at a temperature of 170° C. for 8 minutes to produce a rubber seal having a thickness of 2 mm. The hardness of the obtained rubber seal was measured in accordance with JIS K6253, and the 100% modulus value, tensile strength and elongation were measured in accordance with JIS K6251.

[0080] <Preparation of samples for compression test evaluation>

[0081] An adhesive was applied to a 400 μm thick cold rolled steel sheet (SPCC: Steel Plate Cold Commercial) surface treated with a zinc phosphate treatment agent to a thickness of 3 μm, and dried at room temperature. The adhesive was prepared by diluting 100 parts by mass of a phenolic resin (97 parts by mass of "SIXON (registered trademark) 715A, manufactured by ROHM AND HAAS" and 3 parts by mass of "SIXON (registered trademark) 715N, manufactured by ROHM AND HAAS") with an organic solvent of 440 parts by mass of methyl ethyl ketone and 110 parts by mass of methanol. Next, the blended rubber composition used for the above thermoplastic evaluation was dissolved in an organic solvent and the viscosity was adjusted to about 1000 to 10000 mPa·s, and then applied to the cold rolled steel sheet (coated with the phenolic resin) so that the thickness of the cured rubber layer was 120 μm, and then vulcanized in a 200° C. oven for 3 minutes to prepare a sample for compression test evaluation of a rubber metal laminate. Here, an anti-adhesion layer may be provided as necessary. The prepared samples for compression test evaluation were evaluated by the following evaluation method. The results are shown in Table 1 below.

[0082] <Compression test (overflow) evaluation>

[0083] A mold formed into a ring-shaped convex shape was pressed on the rubber layer of the rubber metal laminate compression test evaluation sample at 100° C. and a pressure of 150 MPa for 5 minutes, and then the state of the rubber layer was evaluated based on the following criteria.

[0084] 5 points: No metal was exposed and almost no rubber flow was observed.

[0085] 4 points: No metal exposure and little rubber flow.

[0086] 3 points: A lot of rubber flow occurs, but not enough to expose the metal.

[0087] 2 points: The flow of rubber is large, but the exposure of metal is small.

[0088] 1 point: The rubber flow is large and the metal exposure is large.

[0089] (Example 2)

[0090] A sample for evaluation of a rubber metal laminate compression test was prepared and evaluated in the same manner as in Example 1 except that 104 parts by mass of carbon black B (SRF carbon black: trade name "HTC#SS", manufactured by Nippon Steel Carbon Co., Ltd.) was used instead of carbon black A. The results are shown in Table 1 below.

[0091] (Example 3)

[0092] A sample for evaluation of a compression test of a rubber-metal laminate was prepared and evaluated in the same manner as in Example 2 except that the thickness of the rubber layer was 80 μm. The results are shown in Table 1 below.

[0093] (Example 4)

[0094] A sample for evaluation of a compression test of a rubber-metal laminate was prepared and evaluated in the same manner as in Example 2 except that the thickness of the rubber layer was 140 μm. The results are shown in Table 1 below.

[0095] (Example 5)

[0096] A sample for compression test evaluation of a rubber-metal laminate was prepared and evaluated in the same manner as in Example 1 except that 56 parts by mass of carbon black C (Semi-Reinforcing Furnace (SRF) carbon black: trade name "ASAHI#50HG", manufactured by Asahi Carbon Co., Ltd.) was used instead of carbon black A. The results are shown in Table 1 below.

[0097] (Example 6)

[0098] A sample for evaluation of a compression test of a rubber-metal laminate was prepared and evaluated in the same manner as in Example 1 except that 90 parts by mass of Carbon Black C was used instead of Carbon Black A. The results are shown in Table 1 below.

[0099] (Example 7)

[0100] A sample for evaluation of a compression test of a rubber-metal laminate was prepared and evaluated in the same manner as in Example 1 except that the blending amount of carbon black A was 181 parts by mass and 10 parts by mass of a plasticizer (trade name "ADK CIZER (registered trademark) RS107", manufactured by ADEKA Corporation). The results are shown in Table 1 below.

[0101] (Example 8)

[0102] A sample for evaluation of the compression test of the rubber-metal laminate was prepared and evaluated in the same manner as in Example 1 except that the compounding amount of carbon black A was 40 parts by mass, carbon black B was used at 60 parts by mass, calcium carbonate (trade name "WHITON SB-Red", manufactured by Beihoku Powder Industry Co., Ltd.) was used at 60 parts by mass, silicon dioxide (trade name "Nipsil (registered trademark) E-74P", manufactured by Tosoh Silica Co., Ltd.) was used at 30 parts by mass, and vulcanizing agent B was not used. The results are shown in Table 1 below.

[0103] (Comparative Example 1)

[0104] A sample for evaluation of a compression test of a rubber-metal laminate was prepared and evaluated in the same manner as in Example 1 except that the blending amount of carbon black A was changed to 45 parts by mass. The results are shown in Table 1 below.

[0105] (Comparative Example 2)

[0106] A sample for evaluation of a compression test of a rubber-metal laminate was prepared and evaluated in the same manner as in Example 1 except that the blending amount of carbon black A was changed to 90 parts by mass. The results are shown in Table 1 below.

[0107] (Comparative Example 3)

[0108] A sample for evaluation of a compression test of a rubber-metal laminate was prepared and evaluated in the same manner as in Example 2 except that the blending amount of carbon black B was 31 parts by mass. The results are shown in Table 1 below.

[0109] (Comparative Example 4)

[0110] A sample for evaluation of a compression test of a rubber-metal laminate was prepared and evaluated in the same manner as in Example 5 except that the blending amount of carbon black C was 30 parts by mass. The results are shown in Table 1 below.

[0111] (Comparative Example 5)

[0112] A sample for evaluation of the compression test of the rubber-metal laminate was prepared and evaluated in the same manner as in Example 1 except that the blending amount of carbon black A was 60 parts by mass, carbon black B was 40 parts by mass, and calcium carbonate (trade name "WHITON SB-Red", manufactured by Beihoku Powder Industry Co., Ltd.) was used. The results are shown in Table 1 below.

[0113] [Table 1]

[0114]

[0115] The details of each component in the above Table 1 are as follows.

[0116] NBR: Nitrile rubber (medium-high nitrile (bound acrylonitrile content 31% or more and less than 36%): trade name "Nipol (registered trademark) DN3350", manufactured by Nippon Ozen Co., Ltd.)

[0117] Carbon black A: Medium particle thermal decomposition (MT: Mdeium Thermal) carbon black (trade name "THERMAX (registered trademark) N990LSR", manufactured by Cancarb Co., Ltd.)

[0118] Carbon black B: medium reinforcement (SRF: Semi-Reinforcing Furnace) carbon black (trade name "HTC#SS", manufactured by Nippon Steel Carbon Co., Ltd.)

[0119] Carbon black C: SRF carbon black (trade name "ASAHI #50HG", manufactured by Asahi Carbon Co., Ltd.)

[0120] Calcium carbonate: Trade name "WHITON SB-Red" (manufactured by Beihoku Powder Chemical Industry Co., Ltd.)

[0121] Silica: Trade name "Nipsil (registered trademark) E-74P" (manufactured by Tosoh Silica Co., Ltd.)

[0122] Plasticizer: Trade name "ADK CIZER (registered trademark) RS107" (manufactured by ADEKA Corporation)

[0123] Zinc oxide: (manufactured by Seido Chemical Industry Co., Ltd.)

[0124] Stearic acid: Trade name "DTST" (manufactured by Miyoshi Oil & Fats Co., Ltd.)

[0125] Antiaging agent: 2,2,4-trimethyl-1,2-dihydroquinoline polymer (trade name "NOCRAC (registered trademark) 810-NA", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)

[0126] Wax: microcrystalline wax (trade name "SUNTIGH (registered trademark) R", manufactured by Seiko Chemical Co., Ltd.)

[0127] Vulcanizing agent A: Colloidal sulfur A (manufactured by Tsurumi Chemical Industries, Ltd.)

[0128] Vulcanizing agent B: 4,4'-dithiodimorpholine (trade name "VULNOC (registered trademark) R", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)

[0129] Vulcanization accelerator A: Tetrabenzylthiuram disulfide (trade name "NOCCELER (registered trademark) TBZTD", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)

[0130] Vulcanization accelerator B: N-cyclohexyl-2-benzothiazolylsulfenamide (trade name "NOCCELER (registered trademark) CZ-P", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)

[0131] As can be seen from Table 1, according to the rubber-metal laminate of the present embodiment, since the 100% modulus value of the rubber layer is 8.5 MPa or more, the flow of the rubber in the compression test is relatively small, and the overflow evaluation score is 4 points or more (Examples 1 to 8). In addition, for carbon black, regardless of whether the medium-grained thermal decomposition carbon black or the medium-reinforcing carbon black is used, the overflow score is 4 points or more (Examples 1 to 6). In addition, even if the thickness of the rubber layer is changed to 80 μm, the flow of the rubber is almost not confirmed in the compression test, and the overflow evaluation score is 5 points (Example 3). Moreover, even if the thickness of the rubber layer is changed to 140 μm, the flow of the rubber is almost not confirmed in the compression test, and the overflow evaluation score is 5 points (Example 4). In addition, in the case of mixing a plasticizer, since the 100% modulus value of the rubber layer is 8.5 MPa or more, the flow of the rubber is almost not confirmed in the compression test, and the overflow evaluation score is 5 points (Example 7). Furthermore, when calcium carbonate and silica were blended, when the 100% modulus value of the rubber layer was 8.5 MPa or more, the flow of the rubber in the compression test was relatively small, and the score of the overflow evaluation was 4 points (Example 8).

[0132] On the other hand, when the 100% modulus value of the rubber layer was less than 8.5 MPa, the flow of the rubber in the compression test was large and the score of the overflow evaluation was 1 to 3 points (Comparative Examples 1 to 5).

[0133] Based on the above results, it can be seen that according to this embodiment, by setting the 100% modulus value of the rubber layer to 8.5 MPa or more and setting the thickness of the rubber layer to 80 μm or more, even when compressive stress acts on the rubber-metal laminate, it is possible to prevent the rubber layer from overflowing, thereby improving the sealing performance of the rubber-metal laminate.

[0134] Industrial Applicability

[0135] As described above, according to this embodiment, there is an effect that a rubber-metal laminate and a gasket can be realized that can prevent the rubber layer from overflowing when compressive stress is applied and have excellent sealing performance of the sealed object member, and the rubber-metal laminate and the gasket of this embodiment are particularly suitable for various gaskets such as cylinder head gaskets, etc. In addition, as a use other than gaskets, such a rubber-metal laminate can also be applied to compressors, water pumps, motors, batteries, power control units, inverter housings, etc.

[0136] Above, an embodiment of the present invention has been described, but the present embodiment of the present invention is not limited by the content of the present embodiment. In addition, the above-mentioned constituent elements include elements that are easily thought of by those skilled in the art, substantially the same elements, and elements of so-called equal scope. Moreover, the above-mentioned constituent elements can be appropriately combined. Moreover, various omissions, substitutions or changes of constituent elements can be performed without departing from the scope of the gist of the above-mentioned embodiment.

Claims

1. A rubber metal laminate, It is characterized in that include: Metal components; and a rubber layer disposed on the metal component, The rubber layer has a 100% modulus value of 8.5 MPa or more based on JIS K6251 and a thickness of 80 μm or more and 200 μm or less, The rubber layer contains 85 parts by mass or more and 250 parts by mass or less of carbon black relative to 100 parts by mass of the rubber component.

2. The rubber-metal laminate according to claim 1, in, In the rubber layer, a 100% modulus value based on JIS K6251 is 10.5 MPa or more.

3. The rubber-metal laminate according to claim 1 or 2, in, In the rubber layer, the elongation value based on JIS K6251 is 100% or more.

4. The rubber-metal laminate according to any one of claims 1 to 3, in, The rubber layer contains 30% by mass or more of carbon black based on the total mass of the rubber layer.

5. The rubber-metal laminate according to any one of claims 1 to 4, in, The metal member and the rubber layer are bonded to each other by at least one adhesive selected from the group consisting of phenolic resins and epoxy resins.

6. The rubber-metal laminate according to any one of claims 1 to 5, in, The rubber layer contains nitrile rubber.

7. A gasket, in, The gasket comprises the rubber-metal laminate according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Method for producing nitrile rubber metal laminate

    CN104289408A

  • Laminate and process for producing same

    CN105431291A

  • Rubber-metal laminate

    US20100086769A1

  • NBR composition for rubber laminated metal

    WO2019102747A1