Selenium and preparation method thereof
By adding ammonia water to the selenite solution and controlling the reaction conditions, high-purity precipitation and high recovery rate of selenium are achieved, which solves the problems of high energy consumption and low recovery rate in the selenium purification process in the existing technology, and improves the purity of selenium. and recovery rates.
Patent Information
- Application Number
- CN202410696128.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-01
AI Technical Summary
The selenium purification process in the prior art has long flow, high energy consumption and low selenium recovery rate, making it difficult to effectively improve the purity and recovery rate of selenium.
After adding ammonia water to the selenite solution, the temperature is raised and an appropriate reducing agent is added to carry out the reduction reaction. The reaction pH endpoint and ammonia water concentration are controlled to achieve high-purity precipitation and high recovery rate of selenium.
The yield and purity of selenium are improved, the waste of selenium element is reduced, the process flow is simplified, and the production efficiency of high-purity selenium is improved.
Smart Images

Figure BDA0004869800830000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-purity selenium preparation, and in particular to selenium and a preparation method thereof. Background Art
[0002] Selenium has the chemical formula Se and a molecular weight of 78.96. Elemental selenium is a red or gray powder, a metalloid with a gray metallic luster. It can be recovered from waste materials such as anode mud of electrolytic copper and flue ash and acid mud of sulfuric acid plants. It can be used as a photosensitive material, a catalyst in the electrolytic manganese industry, an essential nutrient for animals, and a beneficial nutrient for plants.
[0003] However, the purity of selenium currently recovered from waste materials is not high. Therefore, purifying selenium and preparing it into high-purity selenium is a relatively important technical point, which can be used in large quantities in the preparation of downstream products.
[0004] At present, the purification of selenium mainly adopts pyrolysis, such as prior art 1: Chinese patent application CN117049482A discloses a method for preparing 3N selenium from crude selenium, wherein sodium hydroxide solution and hydrogen peroxide are respectively added to the crude selenium raw material to remove soluble impurities, and then vacuum distillation is carried out at a temperature of 650-700°C for purification, and then a mixed salt of sodium nitrate and sodium carbonate is added after melting to carry out a smelting refining reaction, and a 3N selenium product is obtained after slag removal and cooling; for 85%-90% crude selenium raw materials, a "three-stage" integrated selenium purification method of "composite impurity removal + vacuum distillation + smelting refining" is adopted, which can effectively obtain high-quality 3N selenium products in batches.
[0005] However, the method disclosed in the prior art 1 requires one wet process and two fire processes, which has a long process and high energy consumption, and the obtained product only reaches the 3N grade.
[0006] Therefore, it is necessary to study a method with a simple process and capable of preparing high-purity selenium. Based on this, prior art 2: Chinese patent application CN115893330A discloses a method for preparing 6N selenium, which comprises: loading the selenium raw material into a raw material kettle, installing a feeder and a condenser, covering the vacuum gland, and drawing the vacuum degree in the distillation furnace to 0.1-5.0 Pa; turning on the temperature control system, controlling the temperature of the upper heating section to 270-310°C, and the temperature of the lower heating section to 240-270°C, and performing heat preservation distillation; after the insulation is completed, stopping the vacuuming, and filling the distillation furnace with protective gas to restore normal pressure; discharging the molten selenium liquid from the discharge port of the product kettle, and receiving the material with a feed tray to obtain a single-distillation semi-finished product; performing a secondary distillation on the single-distillation semi-finished product to obtain a secondary distillation semi-finished product; S6, granulating and drying the secondary distillation semi-finished product to obtain 6N selenium granules.
[0007] The preparation method disclosed in Prior Art 2 can prepare selenium with a purity of 6N level through a relatively simple process, and has extremely high market application value. However, the ability of Prior Art 2 to prepare selenium with a purity of 6N level is based on the use of a selenium raw material of 4.5N level. Paragraph 0010 of the specification of Prior Art 2 states: "The selenium raw material is a selenium material obtained by reducing a selenious acid solution with formic acid, and then centrifuging, washing, and drying."
[0008] It can be seen that the preparation of 4N grade selenium can be obtained by reducing a selenious acid solution with formic acid. When the applicant tested the method for preparing 4N grade selenium, it was found that the yield of selenium obtained by the method was low, only 30-40%, which would waste a large amount of selenium and have a great impact on the subsequent recovery and treatment of selenium.
[0009] Therefore, the technical problem to be solved by the present invention is: how to prepare high-purity selenium while improving the recovery rate of selenium. Summary of the invention
[0010] One of the purposes of the present invention is to provide a method for preparing selenium, wherein the selenium prepared by the method has a purity of 4N or above, and the recovery rate of the recovered selenium is extremely high, thereby greatly improving the production efficiency of high-purity selenium.
[0011] Another object of the present invention is to provide selenium, which is prepared by the selenium preparation method of the present invention and has a purity of 4N or above, and can be used in the synthesis of various materials or provide better raw materials for further purification of selenium.
[0012] To achieve the above object, the present invention provides a method for preparing selenium, comprising the following steps:
[0013] Step 1: adding ammonia water to the selenious acid solution to obtain a mixed solution;
[0014] Step 2: heating the mixed solution to 90°C-110°C and adding a reducing agent to perform a reduction reaction to obtain a selenium precipitate;
[0015] The concentration of ammonia water in the mixed solution is 3-20g / L.
[0016] Furthermore, the reducing agent is at least one of formic acid, acetic acid, ethanol and oxalic acid.
[0017] It should be noted that the amount of the reducing agent can be adjusted according to the reducing agent used, with the purpose of completely reducing the selenious acid into selenium precipitate by the reducing agent.
[0018] Preferably, the selenious acid solution can be purchased from outside, or prepared by mixing selenium dioxide with water.
[0019] More preferably, the selenious acid solution is prepared from raw material selenium dioxide by the following steps:
[0020] Step a: Selenium dioxide is mixed with water and stirred until completely dissolved, and then solid-liquid separation is performed to obtain selenious acid solution A;
[0021] Step b: treating the selenious acid solution A with resin adsorption to remove mercury in the selenious acid solution A to obtain a selenious acid solution.
[0022] Furthermore, the specific operations of step 2 are:
[0023] The mixed solution is placed in a condensation reflux device and heated to 90-110°C, a reducing agent is added to carry out a reduction reaction, and then solid-liquid separation is performed to obtain selenium precipitate and waste liquid;
[0024] The pH end point of the reaction after adding a reducing agent for reduction reaction is 1.8-2.8.
[0025] More preferably, when the reducing agent is formic acid, the mass ratio of formic acid to selenium dioxide is 0.8-0.9:1.
[0026] Furthermore, the method further comprises step 3: washing the selenium precipitate with pure water until the conductivity is less than 150 us / cm, and drying at a drying temperature of 80° C.-250° C. to obtain selenium powder.
[0027] More preferably, the heating temperature in step 2 is 95-105° C. Using this temperature for the heat preservation reduction reaction treatment can further stabilize the selenium yield.
[0028] More preferably, the reaction pH endpoint of the reduction reaction in step 2 is 2.2-2.5. The use of this reaction pH endpoint can further stabilize the selenium yield.
[0029] The present invention also provides selenium, which is prepared by adopting the above-mentioned method for preparing selenium.
[0030] Beneficial Effects
[0031] Compared with the prior art, the present invention has at least the following advantages:
[0032] (1) The present invention discloses a method for preparing selenium, wherein ammonia water is added before a reducing agent is used to reduce a selenious acid solution. Under the promotion of ammonia water, the yield of selenium is effectively improved and the waste of selenium element is avoided;
[0033] (2) The present invention further improves the yield of selenium by controlling the concentration of aqueous ammonia in the mixed solution;
[0034] (3) The present invention controls the pH endpoint of the reduction reaction, thereby effectively avoiding the decrease in selenium purity and stabilizing the selenium yield. DETAILED DESCRIPTION
[0035] The present invention will be further described below in conjunction with the embodiments, but it does not constitute any limitation to the present invention. Any limited number of modifications made within the scope of the claims of the present invention are still within the scope of the claims of the present invention.
[0036] In order to explain the technical content of the present invention in detail, further description is given below in conjunction with the implementation modes.
[0037] Example 1
[0038] Selenium is prepared by the following steps:
[0039] Step 1: Dissolve 600 g of selenium dioxide in 0.9 L of water and stir until completely dissolved to obtain a selenious acid solution;
[0040] Step 2: Add 2.7 g of aqueous ammonia to the selenious acid solution to obtain a mixed solution;
[0041] Step 3: placing the mixed solution in a condensation reflux device and heating it to 90° C., adding 480 g of formic acid to carry out a reduction reaction until the reaction pH end point is 1.8, and then performing solid-liquid separation to obtain selenium precipitate and waste liquid;
[0042] The selenium precipitate is washed with pure water until the conductivity is less than 150 us / cm, and then dried at a drying temperature of 100° C. to obtain selenium powder.
[0043] Example 2
[0044] Selenium is prepared by the following steps:
[0045] Step 1: dissolving 600 g of selenium dioxide in 0.9 L of water, stirring until completely dissolved, and then performing solid-liquid separation by suction filtration to obtain a selenious acid solution A, and then subjecting the selenious acid solution A to resin adsorption treatment to remove mercury in the selenious acid solution A to obtain a selenious acid solution;
[0046] Step 2: Add 2.7 g of aqueous ammonia to the selenious acid solution to obtain a mixed solution;
[0047] Step 3: placing the mixed solution in a condensation reflux device and heating it to 90° C., adding 480 g of formic acid to carry out a reduction reaction until the reaction pH end point is 1.8, and then performing solid-liquid separation to obtain selenium precipitate and waste liquid;
[0048] The selenium precipitate is washed with pure water until the conductivity is less than 150 us / cm, and then dried at a drying temperature of 100° C. to obtain selenium powder.
[0049] Example 3
[0050] It is generally the same as Example 2, except that the amount of ammonia water added in step 2 is 18 g.
[0051] Example 4
[0052] It is generally the same as Example 2, except that the amount of ammonia water added in step 2 is 9 g.
[0053] Example 5
[0054] It is generally the same as Example 2, except that the reaction pH endpoint in step 3 is 2.9.
[0055] Example 6
[0056] It is generally the same as Example 2, except that the reaction pH end point in step 3 is 1.5.
[0057] Comparative Example 1
[0058] It is generally the same as Example 2, except that the temperature in step 3 is raised to 85°C.
[0059] Comparative Example 2
[0060] It is generally the same as Example 2, except that the amount of ammonia water added in step 2 is 1.8 g.
[0061] Comparative Example 3
[0062] It is generally the same as Example 2, except that the amount of ammonia water added in step 2 is 20 g.
[0063] Comparative Example 4
[0064] The method is generally the same as Example 2, except that step 2 is omitted, ammonia water is not added to the selenious acid solution, and the selenious acid solution is directly subjected to the reduction reaction treatment of step 3.
[0065] The selenium recovery rates and product selenium data of Examples 1-6 and Comparative Examples 1-4 are shown in Table 1;
[0066] The selenium recovery rate = the mass of the selenium powder after drying / the mass of the selenium element in the raw material * 100%, and the purity of selenium is obtained by titration test.
[0067] Table 1 Selenium recovery rate and product selenium purity data of Examples 1-6 and Comparative Examples 1-4 (wherein, the unit of other element impurities except Se is ppm)
[0068]
[0069] According to the results in Table 1, we can see that:
[0070] According to the data comparison between Example 1 and Example 2, in the process of preparing the selenious acid solution, the selenium purity of the selenious acid solution will affect the purity of the final product selenium powder.
[0071] According to the data comparison of Examples 2-4, within the ammonia concentration range defined by the present invention, the selenium yield obtained after the mixed solution is reduced with formic acid will also be affected; within the ammonia concentration range defined by the present invention, the higher the ammonia concentration, the higher the selenium recovery rate;
[0072] However, according to the data of Comparative Examples 2 and 3, when the concentration of ammonia water exceeds the ammonia water concentration range specified by the present invention, the selenium recovery rate will drop significantly. It is speculated that the possible reasons are: the ammonia water concentration used in Comparative Example 2 is too low, and the reduction catalytic effect produced is not obvious, thereby affecting the final selenium recovery rate; and although Comparative Example 3 increases the concentration of ammonia water, as the reduction reaction proceeds, selenious acid is consumed too quickly, the pH rises too quickly, and the rapid change in the pH environment affects the progress of the reduction reaction, thereby affecting the final selenium recovery rate.
[0073] Similarly, according to the data comparison of Examples 2-4, Comparative Example 2, Comparative Example 3 and Comparative Example 4, it can be seen that the technical solution of adding ammonia water as a promoter for the reduction reaction before using formic acid to reduce the selenious acid solution to prepare selenium can greatly improve the recovery rate of selenium.
[0074] According to the data comparison between Example 2 and Comparative Example 1, when the temperature of the reduction reaction is too low, the selenium recovery rate will also decrease.
[0075] The embodiments presented herein are only embodiments selected according to the combination of all possible embodiments. The appended claims should not be limited by the embodiments describing the present invention. Some numerical ranges used in the claims include sub-ranges therein, and the changes in these ranges should also be covered by the appended claims.
Claims
1. A method for preparing selenium, characterized in that: The steps include: Step 1: adding ammonia water to the selenious acid solution to obtain a mixed solution; Step 2: heating the mixed solution to 90°C-110°C and adding a reducing agent to perform a reduction reaction to obtain a selenium precipitate; The concentration of ammonia water in the mixed solution is 3-20g / L.
2. The method for preparing selenium according to claim 1, characterized in that: The reducing agent is at least one of formic acid, acetic acid, ethanol and oxalic acid.
3. The method for preparing selenium according to claim 1 or 2, characterized in that: The selenious acid solution is prepared from raw material selenium dioxide by the following steps: Step a: Selenium dioxide is mixed with water and stirred until completely dissolved, and then solid-liquid separation is performed to obtain selenious acid solution A; Step b: treating the selenious acid solution A with resin adsorption to remove mercury in the selenious acid solution A to obtain a selenious acid solution.
4. The method for preparing selenium according to claim 3, characterized in that: The specific operations of step 2 are: The mixed solution is placed in a condensation reflux device and heated to 90-110°C, a reducing agent is added to carry out a reduction reaction, and then solid-liquid separation is performed to obtain selenium precipitate and waste liquid; The pH end point of the reaction after adding a reducing agent for reduction reaction is 1.8-2.
8.
5. The method for preparing selenium according to claim 4, characterized in that: When the reducing agent is formic acid, the mass ratio of formic acid to selenium dioxide is 0.8-0.9:
1.
6. The method for preparing selenium according to claim 4, characterized in that: The method also includes step 3: washing the selenium precipitate with pure water until the conductivity is less than 150 us / cm, and drying at a drying temperature of 80° C.-250° C. to obtain selenium powder.
7. The method for preparing selenium according to claim 4, characterized in that: The heating temperature in step 2 is 95-105°C.
8. The method for preparing selenium according to claim 4, characterized in that: The reaction pH end point of the reduction reaction in step 2 is 2.2-2.
5.
9. A selenium, characterized in that The selenium is prepared by the method for preparing selenium as described in any one of claims 1 to 7.
Citation Information
Patent Citations
Preparation method of 6N selenium
CN115893330A
Method for preparing 3N selenium from crude selenium
CN117049482A