Desulfurization process of wet-process phosphoric acid

By preparing flotation phosphate tailings into a highly active liquid calcium dihydrogen phosphate desulfurizer for wet phosphoric acid desulfurization, the problems of low activity of calcium sources and entry of magnesium elements in the existing technology are solved, and high-efficiency, low-cost desulfurization is achieved. Wet phosphoric acid desulfurization produces high-purity and high-white clean gypsum.

CN118723951AActive Publication Date: 2024-10-01YIDU XINGFA CHEMICAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410974845.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-01
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The calcium source material used in the existing wet phosphoric acid desulfurization process has low activity and many impurities, resulting in long desulfurization time and poor effect. When the phosphate tailings are directly used for desulfurization, magnesium enters the wet phosphoric acid liquid phase, forming difficult-to-treat Phosphogypsum.

Method used

The flotation phosphate tailings are leached and demagnesized by organic weak acid and then reacted with phosphoric acid to prepare highly active liquid calcium dihydrogen phosphate as a desulfurization agent, which is used to react with wet phosphoric acid to generate high-purity, high-white clean gypsum to avoid by-product phosphorus. Gypsum production.

Benefits of technology

It achieves short desulfurization time and excellent effect, reduces the impurity content in wet phosphoric acid, makes full use of phosphate tailings resources, improves the purity and whiteness of the product, and avoids the formation of phosphogypsum that is difficult to handle.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a wet-process phosphoric acid desulfurization process, and belongs to the technical field of wet-process phosphoric acid desulfurization. The method comprises the following steps: by taking the wet-process phosphorus chemical flotation phosphate tailings as a raw material, leaching with an organic weak acid to remove magnesium, reacting with excessive phosphoric acid under the action of a catalyst, and then carrying out solid-liquid separation to obtain a desulfurizer of which the main component is monocalcium phosphate; and filtering after desulfurization reaction to obtain desulfurized phosphoric acid and high-purity high-whiteness clean gypsum. According to the method, the flotation phosphate tailings are prepared into the desulfurizing agent for wet-process phosphoric acid desulfurization, a new high-valued comprehensive utilization approach is developed for low-added-value solid waste, phosphorus and calcium resources in the phosphate tailings are fully recycled, and economic benefits and social benefits are obvious; the desulfurizer reacts with sulfate radicals in wet-process phosphoric acid to directly generate high-purity and high-whiteness clean gypsum, and generation of a byproduct ardealite which is difficult to treat is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a desulfurization process simultaneously carried out with a method for preparing a wet-process phosphoric acid desulfurizer, and belongs to the technical field of wet-process phosphoric acid desulfurization. Background Art

[0002] At present, the wet phosphoric acid production process in my country mostly uses phosphorus-sulfur mixed acid to decompose phosphate ore, and solid-liquid separation is performed after the reaction to obtain wet phosphoric acid and phosphogypsum. However, due to the characteristics of the wet phosphoric acid production process, in order to ensure the overall phosphorus yield in the production process and generate neat, uniform, and coarse calcium sulfate crystals, the liquid phase sulfate content is often kept appropriately excessive in the production system, resulting in a certain amount of sulfate in the final product phosphoric acid, which can reach 3.0~4.5wt%. The presence of sulfate will affect the quality of downstream terminal products of phosphorus chemical industry. Therefore, removing sulfate from wet phosphoric acid is a necessary process step before producing feed-grade phosphate, industrial-grade ammonium phosphate products, and phosphoric acid purification products. At present, the idea of ​​desulfurization of wet phosphoric acid in industry is to add soluble calcium source to wet phosphoric acid, and remove sulfate by forming calcium sulfate precipitation by the calcium source and sulfate. For example, patent CN104495771A discloses a method for desulfurization of dilute phosphoric acid, in which calcium-containing defluorination slag is added to dilute phosphoric acid for desulfurization; patent CN103754850B discloses a method for reducing the sulfate content in dilute phosphoric acid by dihydrate, in which fertilizer-grade calcium hydrogen phosphate obtained by lime precipitation treatment of phosphorus-containing wastewater is added as a desulfurizer to wet phosphoric acid extraction slurry for desulfurization; patent CN115092898B discloses a method for removing sulfate from wet phosphoric acid by using yellow phosphorus slag, in which yellow phosphorus slag produced as a byproduct in the process of producing yellow phosphorus by electric furnace is re-pulped and added to wet dilute phosphoric acid for desulfurization under the action of an auxiliary agent; patent CN117534046A discloses a method for desulfurization of phosphoric acid by using sludge slag instead of phosphate concentrate, in which the sludge slag is re-pulped and added to wet phosphoric acid for desulfurization. However, the calcium source materials used in these patents are all solid materials with high impurity content and low calcium activity. When used for desulfurization, it will not only lead to a long desulfurization time and poor desulfurization effect, but also cause the soluble impurities in the calcium source materials to enter the wet-process phosphoric acid, thereby reducing the quality of the wet-process phosphoric acid, and the insoluble impurities co-precipitate with calcium sulfate crystals to produce difficult-to-treat phosphogypsum solid waste.

[0003] Phosphorus tailings from wet phosphorus chemical flotation are solid wastes with low phosphorus content generated during the beneficiation process of phosphate ore. Its main components are calcium oxide, magnesium oxide, phosphorus pentoxide, silicon dioxide, etc. 2 O 5The content is 5~8wt%, CaO≥35wt%, MgO≥15 wt%. Phosphorus tailings contain not only soluble calcium elements that can react with sulfate, but also more phosphorus elements, which can not only meet the needs of wet phosphoric acid desulfurization, but also make full use of the phosphorus elements in phosphorus tailings, such as patent CN104555961A discloses a method of defluorination and desulfurization with tailings, directly adding phosphorus tailings in the form of dry ore powder or slurry to wet phosphoric acid or phosphorus-containing wastewater for desulfurization. However, the patent directly uses phosphorus tailings for desulfurization, which not only takes a long time to desulfurize, but also has poor desulfurization effect, and will cause a large amount of magnesium in phosphorus tailings to enter the wet phosphoric acid liquid phase, so that the impurity magnesium content in wet phosphoric acid soars, and silicon enters the solid phase to generate a large amount of difficult-to-handle phosphogypsum. Therefore, phosphorus tailings are not suitable for direct use in wet phosphoric acid desulfurization. Summary of the invention Aiming at the shortcomings of the existing wet phosphoric acid desulfurization technology, the present invention provides a method for preparing a wet phosphoric acid desulfurization agent and a desulfurization process. The process prepares a desulfurization agent from flotation phosphorus tailings for wet phosphoric acid desulfurization, develops a new high-value comprehensive utilization approach for low-value-added solid waste, fully recycles and utilizes phosphorus and calcium resources in the phosphorus tailings, and has obvious economic and social benefits. The liquid desulfurization agent with calcium dihydrogen phosphate as the main component has high calcium element activity, simple composition, few impurities, short desulfurization time, excellent desulfurization effect, and will not increase the content of impurity elements in the wet phosphoric acid. The desulfurization agent reacts with sulfate in the wet phosphoric acid to directly generate high-purity, high-whiteness, clean gypsum, thereby avoiding the generation of by-product phosphogypsum that is difficult to treat.

[0004] The technical scheme of the present invention is as follows: using wet-process phosphorus chemical flotation phosphate tailings as raw materials, after organic weak acid leaching and magnesium removal, reacting with excess phosphoric acid under the action of a catalyst, and then performing solid-liquid separation to obtain a desulfurizer whose main component is calcium dihydrogen phosphate, adding the desulfurizer to wet-process phosphoric acid, filtering after desulfurization reaction to obtain desulfurized phosphoric acid and high-purity, high-white clean gypsum.

[0005] A desulfurization process for wet-process phosphoric acid comprises the following steps: (1) adding wet phosphorus chemical flotation tailings into excess organic weak acid for leaching reaction, filtering after the reaction is completed to obtain filter residue and filtrate; (2) subjecting the filter residue obtained in step (1) to an acid hydrolysis reaction with an excess of phosphoric acid under the action of a catalyst, and performing solid-liquid separation after the reaction is completed, wherein the obtained liquid phase is a desulfurizer whose main component is calcium dihydrogen phosphate; (3) The desulfurizing agent obtained in step (2) is added to wet-process phosphoric acid for desulfurization reaction. After the reaction is completed, desulfurized phosphoric acid and high-purity, high-white clean gypsum are obtained by filtering.

[0006] In the step (1), the phosphate tailings P 2 O 5The content is 5~8wt%, CaO≥35wt%, MgO≥15 wt%.

[0007] The organic weak acid is one or more of benzoic acid, citric acid, oxalic acid, and acrylic acid; the concentration of the organic weak acid is 5-15%.

[0008] Preferably, the concentration of the organic weak acid is 5-10%.

[0009] The mass ratio of phosphate tailings to organic weak acid is 1:2~5, the leaching reaction time is 30~60min, and the leaching reaction temperature is 30~50℃.

[0010] In the step (2), the initial phosphoric acid is P 2 O 5 The industrial phosphoric acid having a sulfate content of 40-45 wt% and a sulfate content of 3.0-4.5 wt% is partially reused in the subsequent continuous circulation production using the desulfurized phosphoric acid obtained in step (3).

[0011] The catalyst is a nitric acid lipid organic substance, including one or more of nitroglycerin, isosorbide dinitrate, isosorbide mononitrate, and pentylenetetrazol.

[0012] The amount of catalyst added is 0.05~0.10 wt% of the mass of phosphoric acid.

[0013] The mass ratio of the filter residue to phosphoric acid is 1:3-6, the acidolysis reaction temperature is 30-75°C, and the acidolysis reaction time is 20-90 minutes. Preferably, the acidolysis reaction temperature is 40-60°C, and the acidolysis reaction time is 20-40 minutes. In the step (3), the amount of desulfurizer added is such that the molar ratio of the calcium content in the desulfurizer to the sulfate content in the wet-process phosphoric acid is 0.9-1.1:1.

[0014] Wet process phosphoric acid P 2 O 5 The content is 40~45wt%, and the sulfate content is 3.0~4.5wt%.

[0015] The desulfurization reaction temperature is 30-70°C, and the desulfurization reaction time is 30-120 minutes. Preferably, the desulfurization reaction temperature is 30-50°C, and the desulfurization reaction time is 30-60 minutes.

[0016] Desulfurized Phosphoric Acid P 2 O 5 The content is 43~48wt%, the sulfate content is 0.1~0.2wt%, the purity of high-purity and high-white clean gypsum is greater than 97%, and the whiteness is greater than 92.

[0017] The beneficial effects of the present invention are: (1) The present invention prepares flotation phosphate tailings into a desulfurizing agent for wet phosphoric acid desulfurization, thus developing a new high-value comprehensive utilization approach for low-value-added solid wastes, with significant social benefits. (2) Phosphate tailings are solid waste by-products of mineral processing. Using them as raw materials to prepare desulfurizers has low costs and can fully recycle the phosphorus and calcium resources in the phosphate tailings, with obvious economic benefits.

[0018] (3) The desulfurizer prepared by the present invention is a liquid desulfurizer. When used for wet phosphoric acid desulfurization, it is a liquid-liquid reaction. The reaction time required is shorter than that of the solid-liquid reaction of a conventional solid desulfurizer. The calcium element in the desulfurizer is highly active and has a good desulfurization effect.

[0019] (4) The desulfurizer prepared by the present invention removes impurities such as magnesium and silicon contained in the phosphate tailings, has a simple composition and few impurities, and will not increase the impurity content in the wet-process phosphoric acid during the desulfurization process.

[0020] (5) The desulfurizer prepared by the present invention does not contain other insoluble impurities and can directly generate high-purity, high-white, clean gypsum by reacting with sulfate in wet-process phosphoric acid, thereby avoiding the generation of by-product phosphogypsum that is difficult to handle. DETAILED DESCRIPTION

[0021] In order to deepen the understanding of the present invention by those skilled in the art, the present invention is further described in detail below in conjunction with specific embodiments. The embodiments are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0022] Example 1-1 A desulfurization process for wet-process phosphoric acid comprises the following steps: (1) P 2 O 5 Phosphate tailings with a content of 5.6wt%, a CaO content of 36.2wt%, and a MgO content of 15.7wt% were added to benzoic acid with a concentration of 6.0% for leaching reaction, the mass ratio of the phosphate tailings to the benzoic acid was controlled to be 1:3, the leaching reaction time was 40min, the leaching reaction temperature was 45°C, and after the reaction was completed, the residue and the filtrate were obtained by filtering. (2) Add the filter residue obtained in step (1) to P 2 O 5 0.05wt% of nitroglycerin by weight of the industrial phosphoric acid is added to industrial phosphoric acid having a sulfate content of 40.9wt% and a sulfate content of 3.8wt%, and the mixture is uniformly mixed and then acid hydrolysis is performed. The mass ratio of the filter residue to the phosphoric acid is controlled to be 1:4, the acid hydrolysis reaction temperature is 60°C, the acid hydrolysis reaction time is 20min, and after the reaction is completed, solid-liquid separation is performed, and the obtained liquid phase is a desulfurizer containing calcium dihydrogen phosphate; (3) Add the desulfurizer obtained in step (2) to P 2 O 5The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 41.4wt% and a sulfate content of 4.1wt%, the amount of desulfurizer added was controlled so that the molar ratio of the calcium content in the desulfurizer to the sulfate content in the wet-process phosphoric acid was 1:1, the desulfurization reaction temperature was 45°C, the desulfurization reaction time was 58min, and after the reaction was completed, it was filtered to obtain P 2 O 5 Desulfurized phosphoric acid with a content of 44.5wt% and a sulfate content of 0.12wt% and clean gypsum with a purity of 97.3% and a whiteness of 93.4.

[0023] Example 1-2 A desulfurization process for wet-process phosphoric acid comprises the following steps: (1) P 2 O 5 Phosphate tailings with a content of 5.2wt%, a CaO content of 35.7wt%, and a MgO content of 16.5wt% were added to citric acid with a concentration of 7.0% for leaching reaction, the mass ratio of the phosphate tailings to the citric acid was controlled to be 1:3.5, the leaching reaction time was 35min, the leaching reaction temperature was 40°C, and after the reaction was completed, the residue and the filtrate were obtained by filtering. (2) Add the filter residue obtained in step (1) to the P obtained in Example 1-1. 2 O 5 isosorbide nitrate of 0.06wt% of the mass of industrial phosphoric acid is added to the desulfurized phosphoric acid with a content of 44.5wt% and a sulfate content of 0.1wt%, and the mixture is evenly mixed and then acid hydrolysis is performed. The mass ratio of the filter residue to the desulfurized phosphoric acid is controlled to be 1:4.5, the acid hydrolysis reaction temperature is 65°C, the acid hydrolysis reaction time is 25min, and after the reaction, solid-liquid separation is performed, and the obtained liquid phase is a desulfurizer containing calcium dihydrogen phosphate; (3) Add the desulfurizer obtained in step (2) to P 2 O 5 The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 40.7wt% and a sulfate content of 4.2wt%, the amount of desulfurizer added was controlled so that the molar ratio of the calcium content in the desulfurizer to the sulfate content in the wet-process phosphoric acid was 1.1:1, the desulfurization reaction temperature was 40°C, the desulfurization reaction time was 55min, and after the reaction was completed, it was filtered to obtain P 2 O 5 Desulfurized phosphoric acid with a content of 44.9wt% and a sulfate content of 0.10wt% and clean gypsum with a purity of 97.2% and a whiteness of 92.8.

[0024] Examples 1-3 A desulfurization process for wet-process phosphoric acid, the process steps are the same as those of Example 1-2, except that 0.09 wt% of pentylenetetrazol in the mass of industrial phosphoric acid is added in step (2). The process also has a significant acid hydrolysis reaction effect, that is, after 22 minutes of acid hydrolysis, the solid-liquid separation obtains a desulfurization agent containing calcium dihydrogen phosphate in the obtained liquid phase.

[0025] (3) Add the desulfurizer obtained in step (2) to P 2 O 5 The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 40.7wt% and a sulfate content of 4.2wt%, the amount of desulfurizer added was controlled so that the molar ratio of the calcium content in the desulfurizer to the sulfate content in the wet-process phosphoric acid was 1.1:2, the desulfurization reaction temperature was 40°C, the desulfurization reaction time was 48min, and after the reaction was completed, it was filtered to obtain P 2 O 5 Desulfurized phosphoric acid with a content of 44.3wt% and a sulfate content of 0.09wt% and clean gypsum with a purity of 97.7% and a whiteness of 93.1.

[0026] Example 2-1 A desulfurization process for wet-process phosphoric acid comprises the following steps: (1) P 2 O 5 Phosphate tailings with a content of 6.6wt%, a CaO content of 36.4wt%, and a MgO content of 16.0wt% are added to acrylic acid with a concentration of 10.0% for leaching reaction, the mass ratio of the phosphorus tailings to the acrylic acid is controlled to be 1:5, the leaching reaction time is 50min, the leaching reaction temperature is 50°C, and after the reaction is completed, filtering is performed to obtain filter residue and filtrate; (2) Add the filter residue obtained in step (1) to the P obtained in Example 1-1. 2 O 5 The content of the filter residue is 44.5wt% and the content of the sulfate is 0.1wt% in desulfurized phosphoric acid, and then the mixture is evenly mixed and then an acid hydrolysis reaction is performed, the mass ratio of the filter residue to the desulfurized phosphoric acid is controlled to be 1:5.5, the acid hydrolysis reaction temperature is 68°C, the acid hydrolysis reaction time is 65min, and after the reaction, solid-liquid separation is performed, and the obtained liquid phase is a desulfurizer whose main component is monocalcium phosphate; (3) Add the desulfurizer obtained in step (2) to P 2 O 5 The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 44.0wt% and a sulfate content of 3.3wt%, the amount of the desulfurizer added was controlled so that the molar ratio of the calcium content in the desulfurizer to the sulfate content in the wet-process phosphoric acid was 1.1:1, the desulfurization reaction temperature was 45°C, the desulfurization reaction time was 120min, and after the reaction was completed, it was filtered to obtain P 2 O 5Desulfurized phosphoric acid with a content of 44.8wt% and a sulfate content of 1.0wt% and clean gypsum with a purity of 97.0% and a whiteness of 93.6.

[0027] Example 2-2 A desulfurization process for wet-process phosphoric acid comprises the following steps: (1) P 2 O 5 Phosphate tailings with a content of 5.8wt%, a CaO content of 36.1wt%, and a MgO content of 15.6wt% were added to oxalic acid with a concentration of 5.0% for leaching reaction, the mass ratio of the phosphate tailings to the oxalic acid was controlled to be 1:2.5, the leaching reaction time was 60min, the leaching reaction temperature was 50℃, and after the reaction was completed, the residue and the filtrate were obtained by filtration. (2) Add the filter residue obtained in step (1) to the P obtained in Example 1-1. 2 O 5 The content of the filter residue is 44.5wt% and the content of the sulfate is 0.1wt% in desulfurized phosphoric acid, and then the mixture is evenly mixed and then an acid hydrolysis reaction is performed, the mass ratio of the filter residue to the desulfurized phosphoric acid is controlled to be 1:6, the acid hydrolysis reaction temperature is 60°C, the acid hydrolysis reaction time is 60min, and after the reaction, solid-liquid separation is performed, and the obtained liquid phase is a desulfurizer whose main component is monocalcium phosphate; (3) Add the desulfurizer obtained in step (2) to P 2 O 5 The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 43.5wt% and a sulfate content of 3.9wt%, the amount of the desulfurizer added was controlled so that the molar ratio of the calcium content in the desulfurizer to the sulfate content in the wet-process phosphoric acid was 1:1, the desulfurization reaction temperature was 45°C, the desulfurization reaction time was 240min, and after the reaction was completed, it was filtered to obtain P 2 O 5 Desulfurized phosphoric acid with a content of 43.9wt% and a sulfate content of 0.4wt% and clean gypsum with a purity of 98.1% and a whiteness of 93.5.

[0028] Example 3 A desulfurization process for wet-process phosphoric acid comprises the following steps: (1) P 2 O 5 The phosphate tailings with a content of 6.1wt%, a CaO content of 35.5wt%, and a MgO content of 15.2wt% and the P obtained in Example 1-1 2 O 5isosorbide mononitrate of 0.07wt% of the mass of industrial phosphoric acid is added to the desulfurized phosphoric acid with a content of 44.5wt% and a sulfate content of 0.1wt%, and the mixture is evenly mixed and then acid hydrolysis is performed, the mass ratio of the phosphorus tailings to the phosphoric acid is controlled to be 1:5, the acid hydrolysis reaction temperature is 72°C, the acid hydrolysis reaction time is 55min, and after the reaction is completed, solid-liquid separation is performed, and the obtained liquid phase is a desulfurizer whose main component is calcium dihydrogen phosphate; (2) Add the desulfurizer obtained in step (1) to P 2 O 5 The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 41.2wt% and a sulfate content of 3.8wt%, the amount of the desulfurizer added was controlled so that the molar ratio of the calcium content in the desulfurizer to the sulfate content in the wet-process phosphoric acid was 0.9:1, the desulfurization reaction temperature was 60°C, the desulfurization reaction time was 60min, and after the reaction was completed, it was filtered to obtain P 2 O 5 Desulfurized phosphoric acid with a content of 45.1wt% and a sulfate content of 0.25wt% and clean gypsum with a purity of 97.8% and a whiteness of 92.5.

[0029] Example 4-1 A desulfurization process for wet-process phosphoric acid comprises the following steps: (1) P 2 O 5 Phosphate tailings with a content of 7.0wt%, a CaO content of 36.7wt%, and a MgO content of 15.4wt% were added to oxalic acid with a concentration of 8.0% for leaching reaction, the mass ratio of the phosphate tailings to the oxalic acid was controlled to be 1:4, the leaching reaction time was 30min, the leaching reaction temperature was 35°C, and after the reaction was completed, the reaction was filtered to obtain a filter residue and a filtrate; (2) Add the filter residue obtained in step (1) to P 2 O 5 The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 42.9wt% and a sulfate content of 3.6wt%, the amount of filter residue added was controlled so that the molar ratio of the calcium content in the filter residue to the sulfate content in the wet-process phosphoric acid was 0.9:1, the desulfurization reaction temperature was 65°C, the desulfurization reaction time was 240min, and after the reaction was completed, it was filtered to obtain P 2 O 5 Desulfurized phosphoric acid with a content of 43.1wt% and a sulfate content of 0.5wt% and phosphogypsum with a purity of 80.3% and a whiteness of 30.4.

[0030] Example 4-2 A desulfurization process for wet-process phosphoric acid comprises the following steps: (1) P 2 O 5Phosphate tailings with a content of 6.4wt%, a CaO content of 35.3wt% and a MgO content of 15.8wt% were added to an organic weak acid with a concentration of 9.0% (acrylic acid and citric acid were mixed in a mass ratio of 1:1) for leaching reaction, the mass ratio of the phosphate tailings to the organic weak acid was controlled to be 1:4.5, the leaching reaction time was 45min, the leaching reaction temperature was 30°C, and after the reaction was completed, the residue and filtrate were obtained by filtering. (2) Add the filter residue obtained in step (1) to P 2 O 5 The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 42.4wt% and a sulfate content of 4.0wt%, the amount of filter residue added was controlled so that the molar ratio of the calcium content in the filter residue to the sulfate content in the wet-process phosphoric acid was 1:1, the desulfurization reaction temperature was 70°C, the desulfurization reaction time was 120min, and after the reaction was completed, filtration was performed to obtain P 2 O 5 Desulfurized phosphoric acid with a content of 42.8wt% and a sulfate content of 1.3wt% and phosphogypsum with a purity of 75.9% and a whiteness of 31.3.

[0031] Example 5-1 A desulfurization process for wet-process phosphoric acid comprises the following steps: P 2 O 5 Phosphate tailings with a content of 6.8wt%, a CaO content of 36.0wt% and a MgO content of 16.1 wt% were added to P 2 O 5 The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 43.1wt% and a sulfate content of 4.2wt%, the amount of phosphorus tailings added was controlled so that the molar ratio of the calcium content in the phosphorus tailings to the sulfate content in the wet-process phosphoric acid was 1.1:1, the desulfurization reaction temperature was 65°C, the desulfurization reaction time was 240min, and after the reaction was completed, it was filtered to obtain P 2 O 5 Desulfurized phosphoric acid with a content of 43.5wt% and a sulfate content of 0.6wt% and phosphogypsum with a purity of 72.6% and a whiteness of 29.8.

[0032] Example 5-2 A desulfurization process for wet-process phosphoric acid comprises the following steps: P 2 O 5 Phosphate tailings with a content of 7.3wt%, CaO content of 35.4wt%, and MgO content of 16.5wt% were added to P 2 O 5The desulfurization reaction was carried out in wet-process phosphoric acid with a calcium content of 40.6wt% and a sulfate content of 4.7wt%, the amount of phosphorus tailings added was controlled so that the molar ratio of the calcium content in the phosphorus tailings to the sulfate content in the wet-process phosphoric acid was 1.1:1, the desulfurization reaction temperature was 70°C, the desulfurization reaction time was 120min, and after the reaction was completed, filtration was performed to obtain P 2 O 5 Desulfurized phosphoric acid with a content of 40.8wt% and a sulfate content of 1.5wt% and phosphogypsum with a purity of 73.4% and a whiteness of 30.3.

Claims

1. A desulfurization process for wet-process phosphoric acid, characterized in that: The following steps are involved: (1) adding the phosphate tailings into an excess of organic weak acid to carry out a leaching reaction, and filtering after the reaction is completed to obtain a filter residue and a filtrate; (2) subjecting the filter residue obtained in step (1) to an acid hydrolysis reaction with an excess of phosphoric acid under the action of a catalyst, and performing solid-liquid separation after the reaction is completed, wherein the obtained liquid phase is a desulfurizer whose main component is calcium dihydrogen phosphate; (3) The desulfurizing agent obtained in step (2) is added to wet-process phosphoric acid for desulfurization reaction. After the reaction is completed, desulfurized phosphoric acid and high-purity, high-white clean gypsum are obtained by filtering.

2. The desulfurization process of wet-process phosphoric acid according to claim 1, characterized in that: In the step (1), the P2O5 content of the phosphate tailings is 5-8wt%, CaO≥35wt%, and MgO≥15wt%.

3. The method for preparing a wet phosphoric acid desulfurization agent and a desulfurization process according to claim 1, characterized in that: In the step (1), the organic weak acid is one or more of benzoic acid, citric acid, oxalic acid, and acrylic acid; and the concentration of the organic weak acid is 5-15%.

4. The desulfurization process of wet-process phosphoric acid according to claim 1, characterized in that: In the step (1), the mass ratio of the phosphate tailings to the organic weak acid is 1:2-5, the leaching reaction time is 30-60 min, and the leaching reaction temperature is 30-50°C.

5. The desulfurization process of wet-process phosphoric acid according to claim 1, characterized in that: In the step (2), the initial phosphoric acid is industrial phosphoric acid having a P2O5 content of 40-45 wt% and a sulfate content of 3.0-4.5 wt%. The desulfurized phosphoric acid obtained in the step (3) is partially reused in subsequent continuous cycle production.

6. The desulfurization process of wet-process phosphoric acid according to claim 1, characterized in that: In the step (2), the catalyst is an organic nitrate lipid, including one or more of nitroglycerin, isosorbide dinitrate, isosorbide mononitrate, and pentylenetetrazol, and the amount of the catalyst added is 0.05-0.10 wt% of the mass of phosphoric acid.

7. The desulfurization process of wet-process phosphoric acid according to claim 1, characterized in that: In the step (2), the mass ratio of the filter residue to the phosphoric acid is 1:3-6, the acidolysis reaction temperature is 30-75°C, and the acidolysis reaction time is 20-90 min.

8. The desulfurization process of wet-process phosphoric acid according to claim 1, characterized in that: In the step (3), the amount of desulfurizer added is such that the molar ratio of the calcium content in the desulfurizer to the sulfate content in the wet-process phosphoric acid is 0.9-1.1:

1.

9. The desulfurization process of wet-process phosphoric acid according to claim 1, characterized in that: In the step (3), the P2O5 content of the wet-process phosphoric acid is 40-45wt%, the sulfate content is 3.0-4.5wt%, the desulfurization reaction temperature is 30-70°C, and the desulfurization reaction time is 30-120min.

10. The desulfurization process of wet-process phosphoric acid according to claim 1, characterized in that: In the step (3), the content of P2O5 in the desulfurized phosphoric acid is 43-48wt%, the content of sulfate is 0.1-0.2wt%, and the purity of the high-purity and high-white clean gypsum is greater than 97%, and the whiteness is greater than 92.

Citation Information

Patent Citations

  • Production technology of food-grade phosphoric acid with hydrochloric acid method

    CN102515134A

  • Phosphorus-containing waste acid extraction separation system and extraction method thereof

    CN112079406A

  • Method for manufacturing of grout chemical using desulfurized gypsum, and grout construction method using the same

    KR102650583B1