Method for preparing carbon material from grain fermented wine byproduct vinasse and application
By subjecting the distiller's grains to primary carbonization and calcination, solvothermal reaction and secondary high-temperature calcination, a carbon material with a multi-level distributed pore structure is prepared, which solves the problems of high recycling cost and environmental pollution of the distiller's grains, and realizes the preparation and production of high-performance battery materials. Resource reuse improves battery performance and stability.
Patent Information
- Application Number
- CN202410781921.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
AI Technical Summary
The recycling cost of distiller's grains is high and there are environmental pollution problems. It is difficult to effectively convert it into high-performance carbon materials with existing technology.
Through primary carbonization and calcination, solvothermal reaction treatment and secondary high-temperature carbonization and calcination, the distiller's grains are prepared into heteroatom-doped carbon materials with a multi-level distributed pore structure. The calcination temperature and heating rate are controlled to improve the conductivity and stability of the material.
It realizes the reuse of resources, reduces the production cost of electrode carbon materials, improves the electrochemical performance of lithium-ion, sodium-ion and potassium-ion batteries, and improves the specific surface area and cycle stability of the material.
Smart Images

Figure CN118723973A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy materials, and in particular to a method for preparing carbon materials by utilizing lees, a byproduct of cereal fermentation wine, and application thereof. Background Art
[0002] Cereal fermented wine, as a major category of wine, is one of the oldest alcoholic beverages. As the largest category of cereal fermented wine, according to the report of International Wine and Spirits Research, Chinese liquor is the best-selling spirit, accounting for more than one-third of global spirits consumption. The production of each ton of fermented wine will produce 2.5-3 tons of by-product lees, so the surge in demand will lead to an increase in lees. The lees are composed of organic acids, starch, protein and lignocellulose. If not handled properly, they will cause environmental risks such as odor and greenhouse gas emissions. In order to alleviate these problems, biorefining is used in the circular bioeconomy. Methods It is a crucial solution to value-add wine lees. Wine lees contain rich bioactive compounds, including a variety of phenolic compounds, and also contain organic acids such as lactic acid and acetic acid, which requires extremely advanced extraction methods to extract the desired target components from wine lees, and the recovery cost is high. The main components of wine lees are cellulose, lignin, etc., which contain a large amount of carbon and rich in proteins and other substances. They contain elements such as N, B, S and P. Studies have found that heteroatoms on carbon materials can improve the reactivity of carbon materials and provide lithium ions (Li) in batteries by modifying functional groups on their surfaces. + ), sodium ion (Na + ) and potassium ions (K + ) provides additional storage sites, thereby significantly improving the electrochemical properties of carbon materials, which makes it possible to convert them into carbon materials and apply them to battery negative electrode materials, and shows excellent potential; the present invention applies distiller's grains to the field of new energy battery electrode material technology, not only to obtain excellent battery performance, but also to comply with the waste recycling advocated by the new energy industry, and to reduce environmental pollution and waste of resources, thus truly "turning waste into treasure" for discarded distiller's grains. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing carbon materials using vinasse, a byproduct of cereal fermentation wine, and its application, so as to solve the problems of recycling vinasse and high cost of raw materials for making carbon materials.
[0004] The technical solution adopted by the present invention to solve the technical problem is a method for preparing electrode materials from wine lees, which includes the following steps.
[0005] S1: Carrying out primary carbonization and calcination of the wine lees to generate a calcined product.
[0006] S2: subjecting the calcined product to a solvent thermal reaction treatment, washing to remove impurities and drying to obtain a precursor material.
[0007] S3: Carry out secondary high-temperature carbonization calcination on the precursor carbon material to obtain a carbon material.
[0008] Furthermore, the distiller's grains described in step S1 are byproducts obtained from the final brewing process of beer, rice wine, sake, etc. using grains as raw materials.
[0009] Furthermore, the solvent described in step S2 is a chemical reagent such as HF, NaOH, etc. that can dissolve SiO2.
[0010] Furthermore, the mass volume ratio of the pre-calcined product to the reaction solvent in step S2 is 1-100 g / 100 ml, and the solvent concentration is 0.5-5 mol / L.
[0011] Furthermore, the heating temperature of the solvent thermal reaction in step S2 is controlled to be 100° C.-190° C., and the reaction time is controlled to be 2 h-24 h.
[0012] Furthermore, the calcination temperature of the initial calcination treatment in step S1 is controlled at 300-800°C, the heating rate is 1-20°C / min, and the constant temperature calcination is maintained for 1-5h.
[0013] Furthermore, the calcination temperature of the secondary calcination treatment in step S3 is controlled at 1000-2500° C., the heating rate is 1-20° C. / min, and the constant temperature calcination is maintained for 1-5 hours.
[0014] The beneficial effects of adopting the above technical solution are:
[0015] (1) The by-product of the winemaking process using grains as raw materials, the lees, is rich in cellulose, lignin, protein and other tissue structures. After carbonization, it can retain a unique microscopic pore structure. The use of lees to prepare carbon materials for recycling can effectively reduce the production cost of electrode carbon materials and promote the development of the new energy battery industry.
[0016] The beneficial effects of adopting the above technical solution are:
[0017] (2) By controlling the reaction reagents, the pore structure, surface functional group structure and element doping of the material can be controlled while removing SiO2, thereby obtaining a heteroatom-doped carbon material with a multi-level distributed pore structure, which has stronger conductivity and promotes the embedding and extraction of ions between carbon layers.
[0018] (3) By controlling the concentration of the reaction solvent, its volume ratio to the material, the reaction time, and the reaction temperature, the efficiency of the solvent thermal reaction is improved, and the calcined product is efficiently converted into a precursor carbon material, thereby ensuring a high yield and element doping rate of the final carbon material.
[0019] (4) A uniform heating rate is used to control the material temperature to the carbonization temperature. The uniform heating rate can ensure that the gas generation that may occur during the carbonization process is reduced, allowing the reaction to proceed more fully and evenly, and reducing the generation of defects and precursor loss. At this rate, the carbon yield is significantly improved, while impurities are removed to improve the purity and stability of the final hard carbon material.
[0020] (5) The secondary calcination temperature is controlled to 1000-2500°C, the degree of graphitization of the material increases, accompanied by the generation of short-range graphite domains and the reduction of defects. The interlayer spacing of the graphite domains becomes narrower as the carbonization temperature increases. The carbon material is calcined at a constant temperature in the temperature range of 1000-2500°C. The lattice spacing is 0.409nm, which is much larger than the graphite spacing (0.340nm). This allows ions to be embedded in the interlayers, and a large number of short-range ordered graphitized domains exist, which can form sufficient closed pores. This step makes the performance of the carbon material more stable.
[0021] Compared with the prior art, the present invention has the following advantages.
[0022] (1) Resource recycling: The present invention utilizes distiller's grains, a by-product of the winemaking process, and converts it into negative electrode materials with high added value, thereby achieving effective resource recycling and reducing waste generation and environmental impact.
[0023] (2) Efficient preparation of negative electrode materials: Through a unique secondary calcination and solvothermal reaction, the carbon yield of the wine lees is guaranteed to be above 50%. The present invention successfully prepares a F / O dual-doped porous carbon matrix; this method can efficiently convert wine lees into precursors of negative electrode materials, providing high-quality starting materials for the battery preparation process.
[0024] (3) High specific surface area: The preparation process uses the method of removing silica to prepare the pore size, which can provide a rich pore size for the carbon material. By controlling the reaction solvent and optimizing the hydrothermal conditions, the specific surface area of the carbon material is increased to 300m 2 g -1 Above, the pore volume reaches 0.6cm 3 g -1 above.
[0025] (4) Improve battery performance: Use hydrofluoric acid as a fluorine-doping agent to increase the fluorine content in carbon materials. By optimizing the HF solvent concentration and the reaction temperature and time, the fluorine content of the carbon material can be increased. Since the F atoms on the carbon material have a strong electronegativity, the F atoms have a strong affinity for Li + 、Na + and K + The adsorption capacity of carbon materials is much stronger than that of carbon materials themselves, which is conducive to the carbon materials to adsorb more Li + 、Na + and K + , thereby improving the electrochemical performance of lithium-ion batteries (LIBs), sodium-ion batteries (SIBs) and potassium-ion batteries (PIBs).
[0026] (5) The fluorine-doped hard carbon material prepared by the present invention has many structural advantages and can obtain excellent electrochemical performance in lithium-ion batteries (LIBs), sodium-ion batteries (SIBs) and potassium-ion batteries (PIBs); the specific capacity of LIBs reaches 1200 mAh g -1 The first cycle coulombic efficiency reaches more than 76%, and the cycle stability reaches more than 1000 cycles; the specific capacity of SIBs reaches 386 mAh g -1 The first cycle coulombic efficiency is above 45%, and the cycle stability is above 1000 cycles; the specific capacity of PIBs is 347 mAh g -1 The first-cycle coulomb efficiency reaches more than 39%, and the cycle stability reaches more than 1,000 cycles; by obtaining stable and excellent electrochemical performance, it lays the foundation for further industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention; in the drawings.
[0028] Figure 1 This is the X-ray diffraction test diagram of the carbon material in Example 1.
[0029] Figure 2 This is a nitrogen absorption and desorption test chart of the carbon material in Example 1.
[0030] Figure 3 This is a scanning electron microscope image of the carbon material in Example 1.
[0031] Figure 4 This is a transmission electron microscope image of the carbon material in Example 1.
[0032] Figure 5 This is a cyclic charge and discharge test diagram of the lithium-ion battery LIBs of Example 4.
[0033] Figure 6This is a cyclic charge and discharge test diagram of the sodium ion battery SIBs of Example 5.
[0034] Figure 7 This is a cyclic charge and discharge test diagram of the potassium ion battery PIBs of Example 6. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The illustrative embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0036] Example 1
[0037] This embodiment is a method for preparing carbon materials using lees, a byproduct of cereal fermentation wine, and the specific steps are as follows.
[0038] Step 1: Carry out the initial carbonization calcination of the liquor lees, raise the temperature to a lower temperature of 700°C at 2°C / min, and continue calcination for 2 hours to generate a calcined product.
[0039] Step 2: subjecting the calcined product to a solvent thermal reaction treatment, using 1 mol / L NaOH for the reaction, with a dosage ratio of 1 g / 100 mL, and the reaction conditions being 120° C. for 18 hours; then filtering and washing the reaction product, and drying it in a vacuum drying oven at 50° C. for 12 hours to obtain a precursor carbon material.
[0040] Step 3: Carry out secondary high-temperature carbonization calcination on the precursor carbon material, increase the temperature to 1000° C. at 5° C. / min, and continue calcination for 2 hours to obtain the carbon material.
[0041] Example 2
[0042] This embodiment is a method for preparing carbon materials using lees, a byproduct of cereal fermentation wine, and the specific steps are as follows.
[0043] Step 1: Carry out the initial carbonization calcination of the beer grains, increase the temperature to a lower temperature of 600°C at 5°C / min, and continue calcination for 1 hour to generate a calcined product.
[0044] Step 2: subjecting the calcined product to a solvent thermal reaction, using 1 mol / L HF for the reaction, with a dosage ratio of 10 g / 100 ml, and the reaction conditions being 180° C. for 12 hours; then filtering and washing the reaction product, and drying it in a vacuum drying oven at 50° C. for 12 hours to obtain a precursor carbon material.
[0045] Step 3: Carry out secondary high-temperature carbonization calcination on the precursor carbon material, increase the temperature to 1200° C. at 5° C. / min, and continue calcination for 3 hours to obtain a carbon material.
[0046] Example 3
[0047] This embodiment is a method for preparing carbon materials using lees, a byproduct of cereal fermentation wine, and the specific steps are as follows.
[0048] Step 1: Carry out the initial carbonization calcination of the rice wine lees, raise the temperature to 700°C at 10°C / min, and continue calcination for 3 hours to generate a calcined product.
[0049] Step 2: subjecting the calcined product to a solvent thermal reaction, using 2 mol / L HF for the reaction, with a dosage ratio of 5 g / 100 ml, and the reaction conditions being 150° C. for 24 hours; then filtering and washing the reaction product, and drying it in a vacuum drying oven at 50° C. for 12 hours to obtain a precursor carbon material.
[0050] Step 3: Carry out secondary high-temperature carbonization calcination on the precursor carbon material, increase the temperature to 1500°C at 10°C / min, and continue calcination for 1 hour to obtain the carbon material.
[0051] Example 4
[0052] The carbon material prepared from the liquor lees in Example 1 is applied to the negative electrode of a lithium-ion battery, and the specific steps are as follows.
[0053] In this example, lithium sheets were used as electrode materials, combined with Celgard 2500 microporous membrane as a separator, and LiPF6 (1 mol) as an electrolyte; the binder polyvinylidene fluoride, the conductive agent acetylene black and the electrode carbon material were mixed evenly in a mass ratio of 8:1:1, and then an appropriate amount of N-methylpyrrolidone was added to make them evenly dispersed; then, the mixture was coated on the current collector copper foil, and after drying, it was roll-pressed; finally, the sample was punched into a disc with a diameter of 14 mm using a puncher for subsequent assembly of lithium-ion batteries (CR2032 type).
[0054] Example 5
[0055] The carbon material prepared from the beer lees in Example 2 is applied to the negative electrode of the sodium ion battery, and the specific steps are as follows.
[0056] In this example, sodium sheets were used as electrode materials, combined with Whatman GF / D glass fibers as separators, and the electrolyte was NaClO4 (1 moL). The binder polyvinylidene fluoride, the conductive agent acetylene black, and the electrode carbon material were mixed evenly in a mass ratio of 8:1:1, and then an appropriate amount of N-methylpyrrolidone was added to make them evenly dispersed; then, the mixture was coated on the current collector copper foil, and after drying, it was roll-pressed; finally, the sample was punched into a disc with a diameter of 14 mm using a puncher for subsequent assembly of sodium-ion batteries (CR2032 type).
[0057] Example 6
[0058] The carbon material prepared from rice wine lees in Example 3 is applied to the negative electrode of a potassium ion battery, and the specific steps are as follows.
[0059] In this example, the counter electrode is a potassium sheet, the diaphragm uses a double-layer Whatman GF / D glass fiber and Celgard2500 microporous membrane, and the electrolyte is KPF6 (1moL). The binder polyvinylidene fluoride, the conductive agent acetylene black and the electrode carbon material are mixed evenly in a mass ratio of 8:1:1, and then an appropriate amount of N-methylpyrrolidone is added to make them evenly dispersed; then, the mixture is coated on the current collector copper foil, and after drying, it is roll-pressed; finally, the sample is punched into a disc with a diameter of 14 mm using a puncher for subsequent assembly of batteries (CR2032 type).
[0060] The carbon material prepared from liquor lees in Example 1 (denoted as FOC) was characterized by the following structure: Figure 1 , Figure 2 , Figure 3 and Figure 4 shown.
[0061] like Figure 1 The figure shows the X-ray diffraction test pattern of the carbon material. Through the X-ray diffractometer, the material composition is analyzed and it is found that there are two broad peaks near 23.6° and 44.3°, corresponding to the (002) crystal plane of the graphite interlayer structure and the (100) crystal plane of graphite. There are no other characteristic peaks, indicating the presence of a small amount of graphitized carbon, which belongs to amorphous carbon; compared with the (002) crystal plane of the standard graphite peak (the standard position is 26°), the (002) peak of FOC shifts to a lower position, which means that it has a larger lattice spacing; this structure is conducive to the deintercalation behavior of its ions in the carbon layer and maintains the stability of the structure.
[0062] like Figure 2The following are (a) nitrogen adsorption-desorption curves of carbon materials; (b) pore size distribution diagram and (c) pore size distribution magnification diagram. The nitrogen adsorption-desorption test (BET) test shows that the specific surface area of the carbon material prepared by doping lees with fluorine is 356.2 m 2 g -1 , indicating that a rich pore structure is generated in the material; in order to explore the pore size distribution in the material, the carbon material was tested for nitrogen adsorption and desorption; Figure 2 As shown in (a), the typical IV isotherm between 0.1-1.0P / P0 is considered to be the characteristic of the coexistence of small pores and mesopores, and the enclosed area of the adsorption-desorption curve is large, indicating that the material has a large specific surface area and rich pores; Figure 2 (b) and (c) show the pore size distribution of carbon materials; the pore size is mainly distributed in the range of 1.2 to 5 nm; the micropores are centered at 1.6 nm and the mesopores are centered at 4.2 nm; therefore, the carbon material prepared by doping lees with fluorine contains more micropores and mesopores, which effectively increases the specific surface area of the material; the rich pore structure and large specific surface area are Li + 、Na + , K + The insertion / extraction of ions provides more active sites and offers additional ion diffusion channels, thereby improving the electrochemical performance of the negative electrode materials.
[0063] Figure 3 SEM images and Figure 4 The transmission electron microscope image shows the surface morphology and microstructure. The amorphous carbon prepared by doping the wine lees with fluorine is mainly composed of carbon nanosheets. Based on this result, the structural changes caused by fluorine doping can be summarized as follows: (1) the spacing between amorphous carbon layers increases; (2) the defect structure of the carbon layer increases; (3) the number of fluorine-containing groups increases; (4) the degree of disorder of the carbon layer structure at the microscopic level increases; these changes are beneficial to Li + 、Na + , K + The deintercalation behavior between carbon layers; therefore, the nanocarbon materials prepared by doping wine lees with fluorine are suitable as electrode materials for lithium ion batteries (LIBs), sodium ion batteries (SIBs) and potassium ion batteries (PIBs).
[0064] Figure 5 for Figure 5 1000 cycle charge and discharge diagram of the lithium-ion battery in implementation case 4 (current density 100 mAh g -1 ),Depend on Figure 5It can be seen that the FOC sample exhibits excellent cycle performance and rate performance after being prepared as a lithium-ion battery. After the performance decay of the first cycle, the subsequent capacity decay maintains a low rate, clearly demonstrating the excellent storage performance of FOC for lithium ions; after 1000 cycles of charge and discharge tests, its capacity is stable at 1209.6mAh g -1 , further verifying its excellent cycle stability; in addition, during the long-term cycle process, the Coulomb efficiency remained at around 99.9% for a long time, further demonstrating the structural stability of FOC click in the long cycle process.
[0065] Figure 6 The charge and discharge diagram of the sodium ion battery in case 5 after 1000 cycles (current density is 100 mAh g -1 ),Depend on Figure 6 It can be seen that FOC exhibits excellent cycling performance when used as a sodium-ion battery electrode; during the first ten cycles, the charge capacity drops rapidly to 423.6 mAh g -1 This phenomenon is mainly due to the formation of the solid electrolyte interface (SEI) layer on the electrode surface and the carbon layer defects for the irreversible Na + The capacity is stabilized at 386.5 mAh g after 1000 cycles. -1 , and the Coulombic efficiency is close to 100%, demonstrating its excellent cycle performance.
[0066] Figure 7 This is the charge and discharge diagram of the potassium ion battery in Example 6 after 1000 cycles (current density is 100 mAh g -1 ),Depend on Figure 7 It can be seen that the first cycle charge capacity is 409.1 mAh g -1 After 1000 cycles, the capacity slowly decreased to 347.2 mAh g -1 , the Coulombic efficiency remains around 100%, showing excellent cycling performance.
[0067] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing carbon materials using lees, a byproduct of cereal fermentation wine, characterized in that: The steps include: S1: performing primary carbonization and calcination on the lees to generate a calcined product; S2: subjecting the calcined product to a solvent thermal reaction treatment, washing to remove impurities and drying to obtain a precursor material; S3: Carry out secondary high-temperature carbonization calcination on the precursor carbon material to obtain a carbon material.
2. The method for preparing carbon material from wine lees according to claim 1, characterized in that: The distiller's grains in step S1 are products obtained from the brewing process of beer, rice wine, sake, etc. using grains.
3. The method for preparing carbon material from wine lees according to claim 1, characterized in that: In the step S1, the calcination temperature of the initial carbonization calcination treatment is controlled to be 300-800°C, the heating rate is 1-20°C / min, and the constant temperature calcination is maintained for 1-5h.
4. The method for preparing carbon material from wine lees according to claim 1, characterized in that: The solvent described in step S2 is a chemical reagent such as HF, NaOH, etc. that can dissolve SiO2.
5. The method for preparing carbon material from wine lees according to claim 1, characterized in that: The mass volume ratio of the calcined product to the reaction solvent in step S2 is 1-100 g / 100 mL, and the solvent concentration is 0.5-5 mol / L.
6. The method for preparing carbon material from wine lees according to claim 1, characterized in that: The solvent thermal reaction temperature in step S2 is controlled to be 100° C.-190° C., and the reaction time is controlled to be 2 h-24 h.
7. The method for preparing carbon material from wine lees according to claim 1, characterized in that: In the step S3, the calcination temperature of the secondary high-temperature carbonization calcination is controlled at 1000-2500° C., the heating rate is 1-20° C. / min, and the constant temperature calcination time is maintained at 1-5 hours.
8. Use of a carbon material prepared from distiller's grains by the method as described in claims 1-7 in the negative electrode of lithium ion batteries, sodium ion batteries and potassium ion batteries.
Citation Information
Patent Citations
Hard carbon material for anode of sodium-ion battery, preparation method of hard carbon material and related sodium-ion battery
CN109678130A
Vinasse type biomass hard carbon material as well as preparation method and application thereof
CN116265391A