Porous carbon material as well as preparation method and application thereof
By using porous carbon materials composed of nickel, nitrogen and carbon elements in lithium-sulfur batteries, the problems of low sulfur utilization and large volume changes in lithium-sulfur batteries are solved, and the high-efficiency cycle stability and rate performance of lithium-sulfur batteries are improved.
Patent Information
- Application Number
- CN202410794509.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-19
AI Technical Summary
Lithium-sulfur batteries have limited application in actual production due to problems such as low sulfur utilization, low conductivity, and large volume changes.
Using porous carbon materials composed of nickel, nitrogen and carbon elements, nano-zinc oxide is prepared as a template through microwave-assisted hydrothermal method, hydrothermal method or calcination method, and urea and nickel chloride hexahydrate are added to furfuryl alcohol to form a three-dimensional interactive structure. The porous carbon material with a connected structure improves the sulfur load and the lithium ion transmission speed.
It significantly improves the cycle stability and rate performance of lithium-sulfur batteries, reduces the diffusion energy barrier of Li+ at the electrochemical interface, promotes liquid-solid phase dynamic conversion, and improves sulfur utilization and the cycle life of the cathode.
Smart Images

Figure CN118723976A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and in particular relates to a porous carbon material and a preparation method and application thereof. Background Art
[0002] Energy is the driving force for the progress and development of human civilization and an important material guarantee for the development of modern industrial technology and social economy. The demand for energy in human society is increasing day by day, and the problem of energy shortage is becoming increasingly prominent. At present, most renewable energy sources are intermittent and require efficient energy storage technology to store and then release energy according to demand. Energy storage technology is the core driving force for the development of renewable energy, and the development of efficient energy storage technology has become one of the research hotspots in the field of energy development.
[0003] Lithium-sulfur batteries have gradually become one of the most promising high-efficiency energy storage technologies due to their advantages such as ultra-high theoretical specific capacity of 1675mAh / g and ultra-high theoretical energy density of 2600Wh / kg. Despite this, lithium-sulfur batteries still face the following problems: (1) The low conductivity of the active material S and its generated discharge products Li2S2 and Li2S leads to low sulfur utilization and poor battery rate performance; (2) The shuttle effect caused by the dissolution and diffusion of polysulfides, that is, the free migration of soluble polysulfides (LiPSs) between the positive and negative electrodes, causes rapid battery capacity decay and low coulombic efficiency; (3) The different densities of S and Li2S lead to large volume changes during charging and discharging. These problems have greatly hindered the application of lithium-sulfur batteries in actual production. Summary of the invention
[0004] In order to overcome at least one of the problems existing in the above-mentioned prior art, the present invention provides a porous carbon material and a preparation method and application thereof.
[0005] To this end, the present invention adopts the following technical solutions:
[0006] A first aspect of the present invention provides a porous carbon material, which is composed of nickel, nitrogen and carbon elements; wherein, in terms of mass percentage, the contents of nickel and nitrogen in the porous carbon material are 1-10% and 0.1-5%, respectively.
[0007] Preferably, the nickel content in the porous carbon material is 2.5-5% by mass.
[0008] The porous carbon material according to the present invention has at least the following beneficial effects: in the porous carbon material, nickel has good dispersion, and the porous carbon material has a three-dimensional interconnected structure, which is physically beneficial to increasing sulfur loading and lithium ion transmission speed.
[0009] The second aspect of the present invention provides a method for preparing the porous carbon material according to the first aspect of the present invention, comprising the following steps:
[0010] 1) preparing nano zinc oxide by microwave-assisted hydrothermal method, hydrothermal method or calcination method;
[0011] 2) Using nano zinc oxide as a template, adding urea and nickel chloride hexahydrate into furfuryl alcohol, heating to react, and calcining to obtain the porous carbon material.
[0012] The method for preparing the porous carbon material, in step 1), the method for preparing nano zinc oxide comprises the following steps:
[0013] Preferably, the anode material of the zinc-manganese battery is dissolved in acetic acid by microwave-assisted hydrothermal method, heated and concentrated to crystallization to obtain zinc acetate, and then methanol is added, microwave heating is performed to a temperature of 110-130°C, the reaction time is 10-15min, centrifugal separation, washing, and drying are performed to obtain the nano zinc oxide. Further preferably, the anode material of the zinc-manganese battery is dissolved in acetic acid by microwave-assisted hydrothermal method, heated and concentrated to crystallization to obtain zinc acetate, and then methanol is added, microwave heating is performed to a temperature of 120-130°C, the reaction time is 10-12min, centrifugal separation, washing, and drying are performed to obtain the nano zinc oxide. Further preferably, the anode material of the zinc-manganese battery is dissolved in acetic acid by microwave-assisted hydrothermal method, heated and concentrated to crystallization to obtain zinc acetate, and then methanol is added, microwave heating is performed to a temperature of 120°C, the reaction time is 10min, centrifugal separation, washing, and drying are performed to obtain the nano zinc oxide.
[0014] Or, preferably, a hydrothermal method is used to dissolve the zinc-manganese battery anode material in acetic acid, heat and concentrate to crystallize to obtain zinc acetate, then add methanol, set the temperature to 50-70°C, stir for 1.5-2.5h, then add potassium hydroxide to react for 0.5-1.5h, centrifuge, wash, and dry to obtain the nano zinc oxide. Or, further preferably, a hydrothermal method is used to dissolve the zinc-manganese battery anode material in acetic acid, heat and concentrate to crystallize to obtain zinc acetate, then add methanol, set the temperature to 60-70°C, stir for 2-2.5h, then add potassium hydroxide to react for 0.5-1.5h, centrifuge, wash, and dry to obtain the nano zinc oxide. Or, further preferably, a hydrothermal method is used to dissolve the zinc-manganese battery anode material in acetic acid, heat and concentrate to crystallize to obtain zinc acetate, then add methanol, set the temperature to 60°C, stir for 2h, then add potassium hydroxide to react for 0.5-1.5h, centrifuge, wash, and dry to obtain the nano zinc oxide.
[0015] Or, preferably, a calcination method is used to dissolve the zinc-manganese battery anode material in acetic acid, heat and concentrate to crystallize to obtain zinc acetate, calcine at 400-480°C for 2-3h, and cool to obtain the nano zinc oxide. Or, further preferably, a calcination method is used to dissolve the zinc-manganese battery anode material in acetic acid, heat and concentrate to crystallize to obtain zinc acetate, calcine at 430-480°C for 2-2.5h, and cool to obtain the nano zinc oxide. Or, further preferably, a calcination method is used to dissolve the zinc-manganese battery anode material in acetic acid, heat and concentrate to crystallize to obtain zinc acetate, calcine at 440°C for 2h, and cool to obtain the nano zinc oxide.
[0016] The preparation method of the porous carbon material is preferably that in step 2), after adding urea and nickel chloride hexahydrate to the furfuryl alcohol, stirring for 30 to 40 minutes, ultrasonicating for 10 to 20 minutes, adding to nano zinc oxide, setting the reaction temperature to 80 to 100°C, the reaction time to 5 to 8 hours, drying, heating to 300°C under gas protection and keeping warm for 5 hours, washing, drying, heating to 550°C and keeping warm for 5 hours, calcining at 900 to 1000°C for 2 to 3 hours, cooling, washing, and drying to obtain the porous carbon material. Further preferably, in step 2), after adding urea and nickel chloride hexahydrate to the furfuryl alcohol, stirring for 30 minutes, ultrasonicating for 10 minutes, adding to nano zinc oxide, setting the reaction temperature to 90-100°C, the reaction time to 5-6 hours, drying, heating to 300°C under argon protection and keeping warm for 5 hours, washing, drying, heating to 550°C under argon protection and keeping warm for 5 hours, calcining at 900°C for 2-3 hours, cooling, washing, and drying to obtain the porous carbon material. Further preferably, in step 2), after adding urea and nickel chloride hexahydrate to the furfuryl alcohol, stirring for 30 minutes, ultrasonicating for 10 minutes, adding to nano zinc oxide, setting the reaction temperature to 90°C, the reaction time to 6 hours, drying, heating to 300°C under argon protection and keeping warm for 5 hours, washing, drying, heating to 550°C under argon protection and keeping warm for 5 hours, calcining at 900-1000°C for 2 hours, cooling, washing, and drying to obtain the porous carbon material.
[0017] The method for preparing the porous carbon material according to the embodiment of the present invention has at least the following beneficial effects:
[0018] The nano zinc oxide particles prepared by microwave-assisted hydrothermal method and hydrothermal method are spherical with a particle size of 5-15nm; the nano zinc oxide prepared by calcination method is rod-shaped with a rod length of 1-2μm and a diameter of about 30nm. Using nano zinc oxide prepared by microwave-assisted hydrothermal method, hydrothermal method or calcination method as a template, urea and nickel chloride hexahydrate are added to furfuryl alcohol, and the prepared porous carbon material has significantly increased pore volume and high specific surface area, and has excellent wettability to lithium-sulfur electrolyte, so it has space and capacity to accommodate more sulfur.
[0019] The third aspect of the present invention provides a porous carbon material positive electrode material, wherein the porous carbon material positive electrode material comprises an electrode membrane and an electrolyte, and the electrode membrane is made of the porous carbon material provided by the first aspect of the present invention.
[0020] Preferably, in the porous carbon material positive electrode material, the thickness of the electrode membrane is 10 to 16 mm, and the mass is 1.5 to 3.0 mg. Further preferably, in the porous carbon material positive electrode material, the thickness of the electrode membrane is 10 to 14 mm, and the mass is 1.5 to 2.0 mg. Even further preferably, in the porous carbon material positive electrode material, the thickness of the electrode membrane is 14 mm, and the mass is 2.0 mg.
[0021] The fourth aspect of the present invention provides a method for preparing the porous carbon material positive electrode material according to the third aspect of the present invention, comprising the following steps:
[0022] 1) adding the porous carbon material into an organic solvent, dispersing it, passing it through an organic filter membrane and vacuum filtering it, drying it, and peeling it off to obtain an electrode membrane;
[0023] 2) Adding a cathode electrolyte dropwise onto the electrode membrane to obtain the porous carbon material positive electrode material.
[0024] Preferably, in step 1), the dispersion time is 1.5 to 2.5 hours, the drying temperature is 60 to 80° C., and the drying time is 12 to 17 hours.
[0025] Preferably, in step 2), the cathode electrolyte is Li2S6 cathode electrolyte, and the sulfur loading of the electrode membrane is 0.5-13 mg / cm 2 Further preferably, in step 2), the cathode electrolyte is Li2S6 cathode electrolyte, and the sulfur loading of the electrode membrane is 0.5-6.2 mg / cm 2 .
[0026] The fifth aspect of the present invention provides a battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode of the battery is the porous carbon material positive electrode material as described in the third aspect of the present invention.
[0027] Preferably, the negative electrode of the battery is a lithium sheet, the separator is a polypropylene separator, and the electrolyte is a lithium-sulfur electrolyte.
[0028] The porous carbon material according to the present invention has at least the following beneficial effects:
[0029] (1) In the porous carbon material of the present invention, nickel has good dispersibility and the porous carbon material has a three-dimensional interconnected structure, which is physically beneficial to increasing the sulfur load and lithium ion transmission rate.
[0030] (2) Using nano zinc oxide prepared by microwave-assisted hydrothermal method, hydrothermal method or calcination method as a template, urea and nickel chloride hexahydrate are added to furfuryl alcohol. The prepared porous carbon material has a significantly increased pore volume and high specific surface area, and has excellent wettability to lithium-sulfur electrolyte, thus having the space and ability to accommodate more sulfur.
[0031] (3) In the preparation method of porous carbon materials, when the calcination temperature is 900°C, the electron transfer rate of the prepared porous carbon material lithium-sulfur battery is the fastest, achieving strong cycle stability and excellent rate performance of the battery.
[0032] (4) Lithium-sulfur batteries made with porous carbon positive electrode materials reduce the Li + The diffusion energy barrier at the electrochemical interface promotes the dynamic transformation of liquid-solid phase in lithium-sulfur batteries. The synergistic effect of the catalytic activity of doped N and Ni jointly improves the reversibility of phase conversion, thereby improving the utilization rate of sulfur and the cycle life of the positive electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The present invention is further described below with reference to the accompanying drawings, embodiments and comparative examples, wherein:
[0034] Figure 1 It is a schematic diagram of the preparation process of the porous carbon material positive electrode material of the present invention.
[0035] Figure 2 Transmission electron microscope (TEM) image, X-ray diffraction (XRD) image, and particle size distribution image of the nano zinc oxide prepared in step 1) of Examples 1, 3, and 5.
[0036] Figure 3 The XRD patterns, scanning electron microscope (SEM) patterns, spherical aberration electron microscope patterns, and energy dispersive X-ray spectroscopy (EDS) images of the porous carbon materials prepared in some embodiments and comparative examples are shown.
[0037] Figure 4 These are the adsorption and electrochemical experimental results of the porous carbon materials of the blank sample, Example 1, Example 3, and Example 5 on lithium polysulfide.
[0038] Figure 5These are the battery performance test results of the batteries composed of the porous carbon materials of Example 1, Example 3, and Example 5.
[0039] Figure 6 The constant potential discharge curve of deposited Li2S and the constant potential charge curve of dissolved Li2S of the battery composed of porous carbon materials of Example 1, Example 3 and Example 5.
[0040] Figure 7 This is a long cycle performance battery test of the batteries composed of the porous carbon materials of Comparative Examples 1 to 12 at a rate of 0.1C.
[0041] Figure 8 The electrochemical impedance spectroscopy (EIS) spectra and cyclic voltammetry (CV) curves of the batteries composed of the porous carbon materials of Comparative Examples 5 to 12 are shown.
[0042] Fig. 9 This is a test diagram of the electrochemical performance of batteries composed of porous carbon materials loaded with different Ni contents in Example 1 and Examples 11 to 14. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below through specific examples and comparative examples, but is not limited to all discussions and data.
[0044] The Li2S6 cathode electrolyte used in the examples and comparative examples is configured as follows:
[0045] 1mol / L Li2S6 cathode electrolyte: 6mmol Li2S and 30mmol sublimed sulfur were added to 6mL 1mol / LLiTFSI-5wt%LiNO3 DOL / DME (volume ratio of 1:1) solution, and magnetically stirred at 60℃ for 24h to prepare 1mol / LLi2S6 cathode electrolyte. The preparation method of 2mol / L Li2S6 cathode electrolyte was the same as above, except that the addition amount of Li2S and sublimed sulfur was doubled.
[0046] Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0047] Embodiment 1:
[0048] 1) Preparation of nano zinc oxide (microwave-assisted hydrothermal method):
[0049] Place the zinc-manganese battery anode material in a 6.26mol / L acetic acid solution, heat in an oil bath at 130℃ and stir for 30min, filter out the insoluble matter, continue heating, concentrate the solution until crystallized, and obtain zinc acetate. Weigh 15g of zinc acetate, place it in a 250mL three-necked flask, add 150mL of methanol, connect the upper interface of the three-necked flask to the lower interface of the condenser, seal the upper interface of the condenser and the other two interfaces of the three-necked flask with a sealing film, heat in a water bath at 60℃, and stir at 200rpm for 2h to obtain zinc acetate-methanol solution. Take 15mL of zinc acetate-methanol solution, transfer it to a 35mL sealed container with a magnetic stirrer, set the microwave program to quickly heat to 120℃, keep it for 10min, take out the container, collect the suspension, and repeat this process many times until the zinc acetate-methanol solution is completely used up. The suspension was centrifuged at a rotation speed of 6000 rpm, washed three times with anhydrous ethanol, and dried in an oven at 60° C. for 12 h to obtain nano zinc oxide.
[0050] 2) Preparation of porous carbon materials:
[0051] 185 mg of urea and 170.56 mg of nickel chloride hexahydrate were added to 2 mL of furfuryl alcohol, magnetically stirred for 30 min, ultrasonicated for 10 min, 5 g of nano zinc oxide prepared in step 1) was added, heated at 90 ° C for 6 h, dried, heated to 300 ° C at a rate of 5 ° C / min in argon, and kept warm for 5 h. The obtained powder was washed with a mixture of deionized water and anhydrous ethanol in a volume ratio of 1:1, dried in an oven at 80 ° C for 12 h, and saturated in argon at a rate of 2 ° C / min. The sample was heated to 550°C at a rate of 10°C / min, kept warm for 5 hours, and then heated to 900°C at a rate of 10°C / min. It was calcined for 2 hours. After cooling to room temperature, the sample was added to a 6.26 mol / L acetic acid solution, sealed, heated to 130°C, and stirred at 500 rpm at 130°C for 36 hours. The suspension was centrifuged at 9000 rpm and washed three times with 6.26 mol / L acetic acid solution. The sample was dried in an oven at 60°C for 12 hours to obtain a porous carbon material.
[0052] 3) Preparation of porous carbon material positive electrode material:
[0053] Add 0.003 g of porous carbon material into anhydrous ethanol and ultrasonically disperse for 2 hours. Pass the solution through an organic filter membrane nylon 66 and vacuum filter, vacuum dry at 60°C for 12 hours, peel off the electrode membrane from the filter membrane, and drop 50 μL of 1 mol / L Li2S6 cathode electrolyte on the electrode membrane to obtain a porous carbon material positive electrode material.
[0054] 4) Preparation of batteries:
[0055] A porous carbon material positive electrode material is used as the positive electrode, a lithium sheet with a diameter of 17 mm is used as the negative electrode, a polypropylene separator is used as the separator, a 1mol / LLiTFSI-2wt%LiNO3 DOL / DME (volume ratio of 1:1) solution is used as the electrolyte, and a standard CR2032 battery shell is used to assemble a button cell, which is recorded as Microwave C-5%Ni.
[0056] Embodiment 2:
[0057] Except for step 3) in the preparation of the porous carbon material positive electrode material, the concentration of the cathode electrolyte dripped on the electrode membrane is 2 mol / L Li2S6, and the remaining steps, amounts, and concentrations are the same as those in Example 1, denoted as Microwave C-5% Ni (high S).
[0058] Embodiment 3:
[0059] 1) Preparation of nano zinc oxide (hydrothermal method):
[0060] The zinc-manganese battery anode material was placed in a 6.26 mol / L acetic acid solution, heated in an oil bath at 130°C and stirred for 30 minutes. After filtering out the insoluble matter, the solution was continued to be heated and concentrated to crystallization to obtain zinc acetate. 15 g of zinc acetate was weighed and placed in a 250 mL three-necked flask, 150 mL of methanol was added, the upper end interface of the three-necked flask was connected to the lower end interface of the condenser, the upper end interface of the condenser and the other two interfaces of the three-necked flask were sealed with a sealing film, heated in a water bath at 60°C, and stirred at a speed of 200 rpm for 2 hours to obtain a zinc acetate-methanol solution, 5 g of potassium hydroxide was added, the sealing film was opened for 5 minutes to prevent flash boiling, the suspension was collected, centrifuged at a speed of 6000 rpm, washed three times with anhydrous ethanol, and dried in an oven at 60°C for 12 hours to obtain nano zinc oxide.
[0061] Except for step 1) the preparation of nano zinc oxide (hydrothermal method) adopts the above-mentioned hydrothermal method, the remaining steps, dosages and concentrations are the same as those in Example 1, which is recorded as Hydrothermal C-5%Ni.
[0062] Embodiment 4:
[0063] Except for step 1) the nano zinc oxide was prepared by using step 1) of Example 3 (hydrothermal method), the remaining steps, dosages and concentrations were the same as those of Example 2, denoted as Hydrothermal C-5% Ni (high S).
[0064] Embodiment 5:
[0065] 1) Preparation of nano zinc oxide (calcination method):
[0066] Place the zinc-manganese battery anode material in a 6.26 mol / L acetic acid solution, heat in an oil bath at 130°C and stir for 30 minutes, filter out the insoluble matter, continue heating, concentrate the solution until crystallized, and obtain zinc acetate. Weigh 1.5 g of zinc acetate and transfer it to a crucible, first heat the muffle furnace to 440°C, then place the crucible in the muffle furnace and calcine for 2 hours, cool, and obtain nano zinc oxide.
[0067] Except for step 1) the preparation of nano zinc oxide (calcination method) adopts the above-mentioned calcination method, the remaining steps, dosages and concentrations are the same as those in Example 1, which is recorded as Calcination C-5%Ni.
[0068] Embodiment 6:
[0069] Except step 1) the nano zinc oxide was prepared by using step 1) of Example 5 (calcination method), the remaining steps, dosages and concentrations were the same as those of Example 2, denoted as Calcination C-5% Ni (high S).
[0070] Embodiment 7:
[0071] Except for step 2) in the preparation of porous carbon material, the calcination temperature for 2 h is 700° C., the other steps, amounts and concentrations are the same as those in Example 1, denoted as Microwave C-5% Ni (700° C.).
[0072] Embodiment 8:
[0073] Except for step 2) in the preparation of porous carbon material, the calcination temperature for 2 h is 800° C., the other steps, amounts and concentrations are the same as those in Example 1, denoted as Microwave C-5% Ni (800° C.).
[0074] Embodiment 9:
[0075] Except for step 2) in the preparation of porous carbon material, the calcination temperature for 2 h is 1000° C., the other steps, amounts and concentrations are the same as those in Example 1, denoted as Microwave C-5% Ni (1000° C.).
[0076] Embodiment 10:
[0077] Except for step 3) in the preparation of the porous carbon material positive electrode material, the amount of cathode electrolyte dripped on the electrode membrane is 4 μL, and the other steps, amounts and concentrations are the same as those in Example 1, which is recorded as Microwave C-5% Ni (low S).
[0078] Embodiment 11:
[0079] Except for step 2) in the preparation of the porous carbon material, the amount of nickel chloride hexahydrate used was 85.28 mg, and the remaining steps, amounts, and concentrations were the same as those in Example 1, denoted as Microwave C-2.5%Ni.
[0080] Embodiment 12:
[0081] Except for step 2) in the preparation of the porous carbon material, the amount of nickel chloride hexahydrate used was 341.12 mg, and the remaining steps, amounts, and concentrations were the same as those in Example 1, denoted as Microwave C-10%Ni.
[0082] Embodiment 13:
[0083] Except for step 2) in the preparation of the porous carbon material, the amount of nickel chloride hexahydrate used was 682.24 mg, and the remaining steps, amounts, and concentrations were the same as those in Example 1, denoted as Microwave C-20%Ni.
[0084] Embodiment 14:
[0085] Except for step 2) in the preparation of the porous carbon material, the amount of nickel chloride hexahydrate used was 1.36 g, and the other steps, amounts and concentrations were the same as those in Example 1, denoted as Microwave C-30%Ni.
[0086] Comparative Example 1:
[0087] The difference from Example 10 is that Comparative Example 1 does not go through step 1) preparation of nano zinc oxide (microwave-assisted hydrothermal method), and no urea, nickel chloride hexahydrate, or nano zinc oxide is added. The other steps, amounts, and concentrations are the same as those of Example 10, and are recorded as Pure C (900° C.).
[0088] Comparative Example 2:
[0089] Except for step 2) in which the temperature of calcination for 2 h in the preparation of the porous carbon material is 700° C., the remaining steps, amounts, and concentrations are the same as those in Comparative Example 1, which is recorded as Pure C (700° C.).
[0090] Comparative Example 3:
[0091] Except for step 2) in which the temperature of calcination for 2 h in the preparation of the porous carbon material is 800° C., the remaining steps, dosages, and concentrations are the same as those in Comparative Example 1, which is recorded as Pure C (800° C.).
[0092] Comparative Example 4:
[0093] Except for step 2) in which the temperature of calcination for 2 h in the preparation of porous carbon material is 1000° C., the remaining steps, dosages and concentrations are the same as those in Comparative Example 1, which is denoted as Pure C (1000° C.).
[0094] Comparative Example 5:
[0095] The difference from Example 10 is that no urea and nickel chloride hexahydrate are added in Comparative Example 5, and the other steps, amounts, and concentrations are the same as those in Example 10, which are recorded as HPC (900° C.).
[0096] Comparative Example 6:
[0097] Except for step 2) in the preparation of porous carbon material, in which the calcination temperature for 2 h is 700° C., the remaining steps, dosages, and concentrations are the same as those in Comparative Example 5, denoted as HPC (700° C.).
[0098] Comparative Example 7:
[0099] Except for step 2) in which the temperature of calcination for 2 hours in the preparation of porous carbon material is 800° C., the remaining steps, dosages and concentrations are the same as those in Comparative Example 5, denoted as HPC (800° C.).
[0100] Comparative Example 8:
[0101] Except for step 2) in the preparation of porous carbon material, in which the calcination temperature for 2 h is 1000° C., the remaining steps, dosages, and concentrations are the same as those in Comparative Example 5, denoted as HPC (1000° C.).
[0102] Comparative Example 9:
[0103] The difference from Example 10 is that no nickel chloride hexahydrate is added in Comparative Example 9, and the other steps, amounts, and concentrations are the same as those in Example 10, which are recorded as HPNC (900° C.).
[0104] Comparative Example 10:
[0105] Except for step 2) in which the temperature of calcination for 2 h in the preparation of the porous carbon material is 700° C., the remaining steps, amounts and concentrations are the same as those in Comparative Example 9, denoted as HPNC (700° C.).
[0106] Comparative Example 11:
[0107] Except for step 2) in which the temperature of calcination for 2 h in the preparation of the porous carbon material is 800° C., the remaining steps, amounts and concentrations are the same as those in Comparative Example 9, denoted as HPNC (800° C.).
[0108] Comparative Example 12:
[0109] Except for step 2) in which the temperature of calcination for 2 h in the preparation of porous carbon material is 1000° C., the remaining steps, dosages and concentrations are the same as those in Comparative Example 9, denoted as HPNC (1000° C.).
[0110] Test method:
[0111] Lithium polysulfide (LiPSs) adsorption experiment:
[0112] In a glove box filled with argon, Li2S and S with a mass ratio of 1:5 were completely dissolved in 1,2-dimethoxyethane (DME) to prepare a 5mmol / L Li2S6 / DME solution. Then, 10mg of porous carbon material was added to 5mL of 5mmo / L Li2S6 / DME solution and allowed to stand for 6h.
[0113] Li2S6 symmetrical battery test:
[0114] A mixed slurry of 75wt% sublimed sulfur, 15wt% porous carbon material and 10wt% polyvinylidene fluoride (PVDF) was uniformly coated on aluminum foil, and a tetraethylene glycol dimethyl ether solution of 0.15mol / L Li2S6, 0.5mol / L LiTFSI and 0.1mol / L LiNO3 was prepared as the electrolyte. When assembling a symmetrical battery, two or more identical electrodes were assembled into a standard 2025-coin battery. 40μL of electrolyte was added to each battery and the electrolyte was charged at 0.2mV s -1 Cyclic voltammetry (CV) measurements were performed on the symmetric cell in the range of -1.0 V to 1.0 V at a scan rate of .
[0115] Li2S deposition experiment:
[0116] 0.4mmol Li2S, 2.8mmol S and 2mmol LiTFSI were dissolved in 2mL tetraethylene glycol dimethyl ether solution and stirred at 50℃ for 8h to prepare 0.2mol / L Li2S8 solution. 20μL Li2S8 solution was dripped into the cathode side. 20μL blank electrolyte without Li2S8 was added to the anode side. The assembled battery was powered on and discharged to 2.06V at a constant current density of 0.112mA, and then kept at a constant potential of 2.05V until the measured current was less than 10 -5 A, The deposition ability of porous carbon materials for Li2S was calculated based on the area under the curve.
[0117] Li2S dissolution experiment:
[0118] The cathode after the Li2S deposition measurement was recovered and reassembled into a new test cell. The new test cell also contained blank electrolyte, Celgard separator and lithium metal foil anode. The assembled test cell was tested at very low current values (about 10 -5 A) to 1.70V, then charge at 2.35V until the test current is less than 10 -5 A, The decomposition ability of porous carbon materials to Li2S is calculated based on the area under the curve.
[0119] Test example:
[0120] (1) Figure 1 Schematic diagram of the preparation process of the porous carbon material positive electrode material of the present invention, as shown in Figure 1 As shown, the zinc-manganese battery anode material is first dissolved in acetic acid to prepare zinc acetate, and then nano zinc oxide is prepared by microwave-assisted hydrothermal method, hydrothermal method or calcination method. With nano zinc oxide, urea and nickel chloride hexahydrate are added to furfuryl alcohol for reaction, and calcined to obtain a porous carbon material.
[0121] (2) The morphology and structure of the nano zinc oxide prepared in step 1) of Examples 1, 3, and 5 were characterized by transmission electron microscopy (TEM) and X-ray diffractometer (XRD). The results are as follows: Figure 2 As shown, Figure 2 (a) is a TEM image of nano zinc oxide (microwave-assisted hydrothermal method) obtained in step 1) of Example 1. Figure 2 (b) is a TEM image of nano zinc oxide (hydrothermal method) obtained in step 1) of Example 3. Figure 2 (c) is a TEM image of nano zinc oxide (calcination method) obtained in step 1) of Example 5. Figure 2 (d) and (e) are the particle size distribution diagrams of nano zinc oxide obtained in Examples 1 and 3. Figure 2 (f) is the XRD spectrum of the nano zinc oxide prepared in Examples 1, 3, and 5. It can be seen from the figure that the nano zinc oxide particles prepared by microwave-assisted hydrothermal method in Example 1 and the nano zinc oxide particles prepared by hydrothermal method in Example 3 are spherical. The particle size of the nano zinc oxide in Example 1 is mainly distributed at about 13 nm, and the particle size of the nano zinc oxide in Example 3 is mainly distributed at about 7 nm. The nano zinc oxide prepared by calcination method in Example 5 is rod-shaped, with a length of 1 to 2 μm and a diameter of about 30 nm. Figure 2 (f) shows that the characteristic peaks of the three samples at 31.8°, 34.4°, 36.3°, 47.5°, 56.6° and 62.9° are well assigned to the (100), (002), (101), (102), (110) and (103) crystal planes of zinc oxide (PDF No:99-0111).
[0122] (3) XRD, scanning electron microscopy (SEM), spherical aberration electron microscopy, and EDS image scanning analysis were performed on some of the prepared porous carbon materials, such as Figure 3 As shown, Figure 3 (a) is the XRD spectrum of the porous carbon materials prepared in Example 1, Example 3, Example 5 and Comparative Example 1, Figure 3 (b) is the XRD spectrum of the porous carbon materials of Examples 1 and 7 to 9, Figure 3 (c) XRD patterns of the porous carbon materials of Examples 1 and 11 to 14, Figure 3 (d), (e), and (f) are SEM and TEM images of the porous carbon materials of Example 1, Example 3, and Example 5, respectively. Figure 3 (g), (h), and (i) are spherical aberration electron microscope images of the porous carbon material of Example 1 at different scales. Figure 3 (j), (k), and (l) are energy dispersive X-ray spectroscopy (EDS) images of different elements in the porous carbon material of Example 1. Figure 3 In (a), in Example 1, Example 3, and Example 5, characteristic diffraction peaks of carbon only appear at 23.6° and 43.4°, and these two diffraction peaks are well attributed to the (002) and (101) crystal planes of carbon, indicating that zinc oxide is no longer present in the final porous carbon material; Figure 3 (b) shows that the (101) peak becomes more intense with the increase of calcination temperature; Figure 3 (c) in the figure, the XRD patterns of the porous carbon materials of Examples 12 to 14, i.e. Microwave C-10% Ni, Microwave C-20% Ni, and Microwave C-30% Ni, showed characteristic peaks of Ni and NiO (see the positions of the yellow arrow and gray arrow in the figure, respectively), while no signals belonging to nickel and its oxides were found in the XRD patterns of the porous carbon materials of Example 1 and Example 11, i.e. Microwave C-5% Ni and Microwave C-2.5% Ni, indicating that nickel is well dispersed in the product; in addition, the porous carbon materials of Example 1 and Example 11 were subjected to inductively coupled plasma optical emission spectroscopy (ICP-OES), and the results showed that the nickel contents were 4.39wt% and 1.85wt%, respectively. Figure 3 In (d), (e), and (f), high-magnification SEM and TEM images show that the porous carbon materials of Example 1, Example 3, and Example 5 have a three-dimensional interconnected structure, which is physically beneficial to increasing the sulfur loading and lithium ion transmission rate. Figure 3 (g) and (h) show that the porous carbon material of Example 1 is loaded with nickel nanocrystals with a size of about 1 to 2 nm, and the lattice spacing of 0.20 nm is very consistent with the (111) crystal plane of nickel. Figure 3 (h) High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) image shows that nickel nanocrystals are surrounded by atomically dispersed single nickel atoms, which are marked as bright spots by red circles, indicating that nickel single atoms and nickel nanocrystals play a synergistic catalytic role during battery cycling. Figure 3The EDS image analysis of (j), (k) and (l) shows that C, N and Ni elements are present in the porous carbon material of Example 1, further confirming the successful preparation of the porous carbon material modified with dispersed nitrogen and nickel atoms.
[0123] (4) Figure 4 The adsorption and electrochemical test results of the porous carbon materials for lithium polysulfide of the blank sample, Example 1, Example 3, and Example 5 are as follows: Figure 4 (a) in the figure shows the Li2S6 adsorption experiment diagrams of the porous carbon materials of the blank sample, Example 1, Example 3, and Example 5 from left to right ("Before" means before the experiment, and "After" means after the experiment). Figure 4 (b) is the UV-visible absorption spectrum of the solution after the porous carbon material of the blank sample, Example 1, Example 3, and Example 5 adsorbed Li2S6. Figure 4 (c) is the cyclic voltammetry (CV) curve of the Li2S6 symmetric battery assembled with the porous carbon material as the positive electrode in Example 1, Example 3, and Example 5, Figure 4 (d) is the Tafel curve of the battery assembled with the porous carbon material as the positive electrode in Example 1, Example 3, and Example 5. Figure 4 (e) and (f) are the EIS spectra of the battery assembled with porous carbon materials as positive electrodes in Example 1, Example 3, and Example 5, and the corresponding Z' and ω -1 / 2 relationship diagram. Figure 4 In (a), the solution colors of Example 1, Example 3, and Example 5 gradually changed from brown to transparent, indicating that they have good adsorption affinity for lithium polysulfide; Figure 4 (b) The UV-visible absorption spectrum shows that compared with the blank sample, the solutions of Example 1, Example 3, and Example 5 have a higher S6 2- The peak intensity decreases; Figure 4 (c) The electrocatalytic effect of the porous carbon materials of Example 1, Example 3, and Example 5 as cathodes in redox reactions was evaluated by cyclic voltammetry of a symmetrical cell. In the range of -0.8V to 0.8V of the CV curve, Example 1, Example 3, and Example 5 all showed redox peaks, among which Example 1 showed the strongest peak current density, indicating that its electrocatalytic activity was the most effective and could promote the rapid catalytic conversion of polysulfides. Figure 4 The Tafel curve (d) shows that the potential and exchange current density of the porous carbon material in Example 1 are the highest, indicating that the monodisperse 5% Ni coordinated with nitrogen in the porous carbon material in Example 1 promotes the dynamic transformation of liquid-solid phase in the lithium-sulfur battery; Figure 4(e) Electrochemical impedance spectroscopy (EIS) shows three similar semicircles, indicating that the charge transfer resistance capabilities of the porous carbon materials of Example 1, Example 3, and Example 5 are similar; at the same time, Figure 4 Figure (e) infers the diffusion coefficient of lithium ions, such as Figure 4 As shown in (f), as the slope value decreases, the conductivity of lithium ions becomes higher and higher. The slope values of Example 1, Example 3, and Example 5 are 4.09, 9.28, and 8.87, respectively, which indicates that the lithium ion diffusion rate in Example 1 is faster than that in Example 3 and Example 5.
[0124] (5) Figure 5 The battery performance test results of the batteries composed of porous carbon materials of Example 1, Example 3 and Example 5 are as follows: Figure 5 (a) to (c) are cyclic voltammetry (CV) curves of the porous carbon materials of Example 1, Example 3, and Example 5 at different scanning rates, respectively. Figure 5 (d) is the first cycle charge-discharge curve of the porous carbon materials of Example 1, Example 3, and Example 5 at a rate of 0.05C. Figure 5 (e) is a cycle performance diagram of the porous carbon materials of Example 1, Example 3, and Example 5 at a rate of 0.1C. Figure 5 (f) is a cycle performance diagram of the porous carbon materials of Example 1, Example 3, and Example 5 at different rates in the range of 0.1C to 3C. Figure 5 (g) is a long cycle performance diagram of the porous carbon materials of Example 1, Example 3, and Example 5 at 1C rate and high sulfur loading. Figure 5 (h) is the long cycle performance diagram of the porous carbon materials of Example 1, Example 3, and Example 5 at 1C rate and ultra-high sulfur loading. Figure 5 From (a) to (c) in the figure, it can be seen that typical anodic peaks (A, B) and cathodic peaks (C, D) appear in Examples 1, 3 and 5. The reaction process represented by each peak is
[0125] A: 4Li2S-6e - →S4 2- +8Li +
[0126] B:2S4 2- -4e - →S8
[0127] C: S8+4e - →2S4 2-
[0128] D: S4 2- +6e - +8Li +→4Li2S
[0129] At the same scan rate, the maximum current density of Example 1 at peak B and peak C is higher than that of Example 3 and Example 5, indicating that the porous carbon material of Example 1 can better promote the formation and decomposition of insulator sulfur, which is of great significance to the different phase transformation processes of sulfur and polysulfide. In addition, the slope values of the anode peaks A, B and the cathode peaks C, D of Example 1 are higher than the peak slope values of Example 3 and Example 5, indicating that the Li + The transmission is the easiest. According to the Randles-Sevcik equation, the calculation equation Li + The diffusion coefficient (D Li+ ), D of cathode of Example 1 Li+ The highest, explaining that the porous carbon material of Example 1 has a unique three-dimensional through and interconnected hierarchical pore structure, which reduces the Li + The diffusion energy barrier at the electrochemical interface and the synergistic effect of the catalytic activity of doped N and Ni together improve the reversibility of the phase transformation, thereby increasing the sulfur utilization and the cycle life of the cathode. Figure 5 Figure (d) shows the first cycle voltage curves of the batteries of Example 1, Example 3, and Example 5 at 0.05C rate within the voltage window of 1.7-2.8V, compared with the battery of Example 5 (1208mA hg -1 ) and Example 3 battery (833mA hg -1 ), the charge and discharge curves of the battery in Example 1 show lower charge overpotential and voltage hysteresis, while achieving a higher specific capacity (1261 mA hg -1 ), in the curve of Example 1, the high utilization rate and high retention rate of the high platform discharge capacity indicate that the diffusion of polysulfides in the lithium-sulfur battery is suppressed, while the high retention rate of the low platform discharge capacity indicates that the captured polysulfides are more thoroughly converted. Figure 5 From (e) in the figure, it can be seen that the sulfur loading is 6.2 mg cm -2 When the initial discharge capacity of the battery in Example 1 is 1095 mA hg -1 ) than Example 3 (834mA hg -1 ), Example 5 (1004 mA hg -1 ) is high because the porous carbon material of Example 1 has larger pores and can accommodate more actual sulfur loading. Figure 5 From (f) in the figure, it can be seen that the sulfur loading is 6.2 mg cm -2 When the discharge rate is from 0.1C to 3C, the battery of Example 1 shows a higher discharge capacity than the batteries of Example 3 and Example 5. Figure 5From (g), it can be seen that the batteries of Example 1, Example 3, and Example 5 have a rate of 6.2 mg cm at 1C. -2 When the sulfur loading amount is high, the battery can still output an extraordinary capacity after 500 cycles, especially the battery in Example 1. Figure 5 As shown in (h), the batteries of Example 1, Example 3, and Example 5 have a rate of 12.4 mg cm at 1C. -2 When the sulfur loading amount is high, the specific capacity is still maintained at a high level after 200 cycles, especially the battery of Example 1.
[0130] (6) Figure 6 The constant potential discharge curve of deposited Li2S and the constant potential charge curve of dissolved Li2S of the battery composed of the porous carbon material of Example 1, Example 3 and Example 5 are shown, wherein: Figure 6 (a) to (c) are constant potential discharge curves. Figure 6 (d) to (f) are constant potential charging curves. Figure 6 Obvious Li2S deposition peaks appeared in (a) to (c), among which Example 1 showed the highest current density and charging capacity, indicating that the reduction of polysulfide in Example 1 was enhanced and promoted. Figure 6 As can be seen from (d) to (f) in the figure, in the reverse Li2S decomposition reaction, Example 1 also exhibits the highest current density and discharge capacity. The results show that Example 1 is also highly efficient in promoting the Li2S oxidation reaction. The micropores and mesopores in Example 1 can provide abundant active sites for the adsorption of polysulfides and provide a high specific surface area to enhance the contact between carbon and polysulfides. Due to the synergistic effect of multiple interactions, Example 1 exhibits extremely strong Li2S nucleation and decomposition kinetics, verifying the bidirectional catalytic activity in the redox reaction of polysulfides.
[0131] (7) Figure 7 The long cycle performance battery test of the battery composed of the porous carbon material of Comparative Examples 1 to 12 at a rate of 0.1C, wherein: Figure 7 (a) is the long cycle performance diagram of comparative examples 1 to 4, Figure 7 (b) is the long cycle performance diagram of Comparative Examples 5 to 8, Figure 7 (c) is the long cycle performance diagram of comparative examples 9 to 12. Figure 7 As shown in Figures (a) and (b), at 0.5 mg cm -2 Sulfur loading, at 0.1C rate, continuous cycle 500 times, the specific capacity of the battery of comparative examples 5 to 8 is higher than that of comparative examples 1 to 4 at the same calcination temperature; Figure 7 As shown in Figures (b) and (c), at 0.5 mg cm -2With respect to sulfur loading, the specific capacity of the batteries of Comparative Examples 9 to 12 after 500 continuous cycles at a rate of 0.1C is generally higher than that of Comparative Examples 5 to 8 at the same calcination temperature, and the specific capacity of the batteries is the largest when the calcination temperature is 900°C.
[0132] (8) Figure 8 The electrochemical impedance spectroscopy (EIS) spectra and CV curves of the batteries composed of the porous carbon materials of Comparative Examples 5 to 12 are shown in FIG. Figure 8 (a) is the EIS spectrum of Comparative Examples 5 to 8, Figure 8 (b) is the EIS spectrum of Comparative Examples 9 to 12, Figure 8 (c) is the CV curve of Comparative Examples 5 to 8, Figure 8 (d) in the figure is the CV curve of comparative examples 9 to 12. Figure 8 Compared with (a) and (b), the electrochemical impedance of comparative examples 9 to 12 is significantly reduced, indicating that nitrogen doping can effectively promote the rapid transfer of electrons, and when the calcination temperature is 900°C, the electron transfer speed is the fastest. Figure 8 Compared with (c) and (d), more obvious redox peaks and higher redox currents appear in Comparative Examples 9 to 12, indicating that the introduction of nitrogen can effectively promote the catalytic conversion kinetic reaction of polysulfides.
[0133] (9) Fig. 9 The electrochemical performance test diagram of the battery composed of porous carbon materials with different Ni content loadings in Example 1 and Examples 11 to 14 is shown in FIG. Fig. 9 (a) is a cycle performance diagram of a battery composed of porous carbon materials prepared in Example 1 and Examples 11 to 14 at a rate of 0.1C, Fig. 9 (b) is the CV curve of the battery composed of the porous carbon material prepared in Example 1 and Examples 11 to 14, Fig. 9 (c) is the EIS spectrum of the battery composed of the porous carbon material prepared in Example 1 and Examples 11 to 14. Fig. 9 As shown in (a), the batteries of Examples 1 and 11-12 have a rate of 0.1C and a rate of 0.5 mg cm -2 When the sulfur loading amount is increased, the specific capacity is still relatively high after 200 cycles, especially the battery of Example 1, while the specific capacity of Examples 13 to 14 is relatively low. Fig. 9 As can be seen from (b), the charge and discharge platforms of the batteries of Examples 1 and 11 to 12 are obvious, but those of Examples 13 to 14 are not obvious. Fig. 9 As can be seen from (c) in the figure, the electrochemical impedances of Example 1 and Examples 11 to 12 are relatively small, especially the battery of Example 1, while the electrochemical impedances of Examples 13 to 14 are relatively large.
Claims
1. A porous carbon material, It is characterized in that The porous carbon material is composed of nickel, nitrogen and carbon elements; Wherein, the contents of nickel and nitrogen in the porous carbon material are 1-10% and 0.1-5% respectively, in terms of mass percentage.
2. The porous carbon material according to claim 1, It is characterized in that Calculated by mass percentage, the nickel content in the porous carbon material is 2.5-5%.
3. The method for preparing a porous carbon material according to any one of claims 1 or 2, It is characterized in that The following steps are involved: 1) preparing nano zinc oxide by microwave-assisted hydrothermal method, hydrothermal method or calcination method; 2) Using nano zinc oxide as a template, adding urea and nickel chloride hexahydrate into furfuryl alcohol, heating to react, and calcining to obtain the porous carbon material.
4. The method for preparing the porous carbon material according to claim 3, It is characterized in that In step 1), the preparation method of nano zinc oxide comprises the following steps: The zinc-manganese battery anode material is dissolved in acetic acid by microwave-assisted hydrothermal method, heated and concentrated to crystallize to obtain zinc acetate, and then methanol is added and microwave-heated to a temperature of 110-130° C. for a reaction time of 10-15 min, centrifuged, washed, and dried to obtain the nano zinc oxide. Alternatively, a zinc-manganese battery anode material is dissolved in acetic acid by a hydrothermal method, heated and concentrated to crystallize to obtain zinc acetate, and then methanol is added, the temperature is set to 50-70° C., stirred for 1.5-2.5 hours, and then potassium hydroxide is added to react for 0.5-1.5 hours, centrifuged, washed, and dried to obtain the nano zinc oxide; Alternatively, a calcination method is adopted to dissolve the zinc-manganese battery anode material in acetic acid, heat and concentrate it to crystallize to obtain zinc acetate, calcine it at 400-480° C. for 2-3 hours, and cool it to obtain the nano zinc oxide.
5. The method for preparing the porous carbon material according to claim 3, It is characterized in that In step 2), after adding urea and nickel chloride hexahydrate to the furfuryl alcohol, stirring for 30 to 40 minutes, ultrasonicating for 10 to 20 minutes, adding to nano zinc oxide, setting the reaction temperature to 80 to 100° C., the reaction time to 5 to 8 hours, drying, heating to 300° C. under gas protection and keeping warm for 5 hours, washing, drying, heating to 550° C. and keeping warm for 5 hours, calcining at 900 to 1000° C. for 2 to 3 hours, cooling, washing, and drying to obtain the porous carbon material.
6. A porous carbon material positive electrode material, It is characterized in that It comprises an electrode membrane and an electrolyte, wherein the electrode membrane is made of the porous carbon material according to any one of claims 1 or 2.
7. The porous carbon material positive electrode material according to claim 6, It is characterized in that The electrode membrane has a thickness of 10 to 16 mm and a mass of 1.5 to 3.0 mg.
8. The method for preparing a porous carbon material positive electrode material according to any one of claims 6 or 7, It is characterized in that The following steps are involved: 1) adding the porous carbon material into an organic solvent, dispersing it, passing it through an organic filter membrane and vacuum filtering it, drying it, and peeling it off to obtain an electrode membrane; 2) Adding a cathode electrolyte dropwise onto the electrode membrane to obtain the porous carbon material positive electrode material.
9. A battery, It is characterized in that The battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode of the battery is the porous carbon material positive electrode material according to any one of claims 6 or 7.
10. The battery according to claim 9, It is characterized in that The negative electrode of the battery is a lithium sheet, the diaphragm is a polypropylene diaphragm, and the electrolyte is a lithium-sulfur electrolyte.
Citation Information
Patent Citations
Method for recovering metal through purified flue gas of scrap alkaline zinc-manganese battery
CN101792861A
Preparation method of nanometer ZnO for lithium ion battery cathode material
CN106542567A
Metallic nickel-nitrogen doped porous carbon materials, preparation method and application of metallic nickel-nitrogen doped porous carbon materials
CN106862589A
Method for preparing nitrogen-doped porous carbon material by using nano zinc oxide
CN110723719A
Method for preparing porous carbon material by utilizing nano zinc oxide template
CN110734047A
Cited By
Zinc-air battery integrated negative electrode and preparation method and application thereof
CN119517944A