Modified basalt-coated UiO-66 composite material as well as preparation method and application thereof
The modified basalt@UiO-66 composite addresses the high cost and performance limitations of UiO-66 by combining K2O-modified basalt nanofibers with UiO-66, resulting in enhanced CO2 adsorption capacity and selectivity for large-scale industrial use.
Patent Information
- Application Number
- CN202411379331.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-06
AI Technical Summary
The high synthesis cost and limited CO2 adsorption capacity and selectivity of UiO-66 material hinder its large-scale application in carbon capture technologies.
A modified basalt@UiO-66 composite material is developed, where K2O-modified basalt nanofibers with a diameter of 15-25 nm are combined with UiO-66, enhancing the specific surface area and pore volume through a series of preparation steps including grinding, etching, and impregnation with zirconium chloride and amino groups.
The composite material achieves high CO2 adsorption capacity and selectivity, reducing production costs and enabling large-scale industrial application.
Smart Images

Figure CN119075944A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of flue gas CO2 capture, and in particular relates to a modified basalt@UiO-66 composite material and a preparation method and application thereof. Background Art
[0002] Energy consumption has surged in recent years and carbon dioxide emissions are about to reach their peak. In order to achieve climate goals, carbon emission reduction will be the focus of work in the coming years.
[0003] Afforestation is a commonly used method for carbon reduction, but its potential is limited and it is difficult to meet such a large-scale carbon reduction demand. Therefore, the development of efficient and scalable carbon capture technology has become a top priority. Among the many carbon capture technologies, the adsorption method uses the van der Waals force or chemical bond adsorption of porous materials to separate CO2 from mixed gases. It is divided into one-time adsorption technology, atmospheric pressure cycle adsorption / desorption technology and pressure swing adsorption technology. The amount of adsorbent required for the one-time adsorption technology is huge, which incurs huge costs, while the operating cost of the pressure swing adsorption technology is relatively high. The atmospheric pressure cycle adsorption / desorption technology has the advantages of low cost, simple equipment and operation, and broad application prospects.
[0004] The core of adsorption technology is adsorbent. Among many adsorbents, MOFs material UiO-66 has an unusually developed pore structure, huge specific surface area and high stability, and is particularly suitable for carbon dioxide adsorption. However, the synthesis cost of UiO-66 material is relatively high, and the adsorption capacity and selectivity of CO2 still need to be improved, which limits its large-scale application. If a widely available and inexpensive material can be used to composite with UiO-66 material, the cost of UiO-66 composite material can be greatly reduced while the adsorption capacity and selectivity of CO2 can be improved, it will lay the foundation for the industrial application of UiO-66 material. Summary of the invention
[0005] In view of the fact that the UiO-66 material has a high synthesis cost and its CO2 adsorption capacity and selectivity still need to be improved, which limits its large-scale application, the present invention provides a modified basalt with a wide source, low price and good adsorption performance, which is composited with the UiO-66 material to achieve high adsorption performance and mechanical stability for CO2.
[0006] In order to solve the problems of the prior art, the technical solution adopted by the present invention is:
[0007] A modified basalt@UiO-66 composite material, wherein the modified basalt is K2O-modified basalt nanofiber with a diameter of about 15-25 nm, the mass ratio of K element to basalt in the modified basalt is 1:4, and the mass ratio of the modified basalt to UiO-66 is (0.2-0.4):1.6.
[0008] Furthermore, the specific surface area of the modified basalt@UiO-66 composite material is 936-1023m 2 / g, pore volume is 0.72-0.76m 3 / g.
[0009] The preparation method of the modified basalt is as follows:
[0010] Step 1, fully grinding basalt in a corundum crucible, adding potassium nitrate, and then melting the mixture at a melting temperature to obtain K2O-modified molten basalt, using porous anodized aluminum as a template, and using a pulse jet method to spray the K2O-modified molten basalt into the alumina template to form nanofibers with a rough surface in the alumina template;
[0011] Step 2: using a NaOH solution of a certain concentration to etch away the alumina template and the silicon oxide, aluminum oxide and other components in the basalt, and strengthening the surface alkalinity of the nanofibers to prepare K2O-modified basalt nanofibers with nanopores.
[0012] A method for preparing a modified basalt@UiO-66 composite material comprises the following steps:
[0013] Step 1, fully grinding basalt in a corundum crucible, adding potassium nitrate, and then melting the mixture at a melting temperature to obtain K2O-modified molten basalt, using porous anodized aluminum as a template, and using a pulse jet method to spray the K2O-modified molten basalt into the alumina template to form nanofibers with a rough surface in the alumina template;
[0014] Step 2: using a NaOH solution of a certain concentration to etch away the alumina template and the silicon oxide, aluminum oxide and other components in the basalt, and strengthening the surface alkalinity of the nanofibers to prepare K2O-modified basalt nanofibers with nanopores;
[0015] Step 3, using a Venturi dust removal method to impregnate zirconium chloride into the K2O-modified basalt nanofibers prepared in step 2, the specific operation is as follows: placing the K2O-modified basalt nanofibers in the feed hopper of the Venturi dust collector, the K2O-modified basalt nanofibers are dispersed and accelerated by the high-speed airflow in the air inlet pipe after being fed, and then enter the throat along the contraction tube, the zirconium chloride solution is sprayed from the nozzles distributed in an annular manner around the throat, atomized and accelerated by the high-speed airflow, and the zirconium chloride droplets are fully collided and impregnated with the K2O-modified basalt nanofibers, and then enter the cyclone separator along the diffusion tube and the connecting tube to complete gas-solid separation;
[0016] Step 4, drying the solid separated in step 3, and then treating it at high temperature in a tube furnace for 4 hours to obtain zirconium chloride and amino-modified K2O-modified basalt nanofibers;
[0017] Step 5, dissolving the zirconium chloride and amino-modified K2O-modified basalt nanofibers obtained in step 4 in a DMF solvent with zirconium chloride and terephthalic acid in a certain mass ratio, transferring to a reactor, reacting at 150°C for 24h, and after cooling, washing the precipitate with DMF and ethanol for 3 times, and drying at 160°C to obtain the final modified basalt@UiO-66 composite material.
[0018] Furthermore, in step 1, the mass ratio of K element in potassium nitrate to basalt is 1:4, the melting temperature is 1500° C., and the pulse jet method is a method of mixing and jetting compressed air at 1500° C. and K2O-doped molten basalt, and the pressure of the compressed air is 10 atm;
[0019] Furthermore, the concentration of the NaOH solution in step 2 is 10wt%, and the treatment time is 1h;
[0020] Furthermore, the speed of the high-speed airflow in the air inlet pipe in step 3 is 40 m / s, the diameter ratio of the throat pipe to the air inlet pipe is 1:2, and the feed mass ratio of zirconium chloride to nanofibers is 3:8;
[0021] Furthermore, the drying temperature in step 4 is 120° C., the temperature of the high temperature treatment in the tube furnace is 400° C., and the atmosphere is a mixed atmosphere of ammonia:nitrogen=1:9;
[0022] Furthermore, the mass ratio of the modified basalt nanofibers to zirconium chloride and terephthalic acid (H2BDC) in step 5 is (0.2-0.4):1.4:1.
[0023] Application of modified basalt@UiO-66 composite material for adsorption of CO2.
[0024] Beneficial effects: Compared with the prior art, the modified basalt@UiO-66 composite material of the present invention and its preparation method and application have the following advantages: (1) The modified basalt in the composite material is K2O-modified basalt nanofiber prepared by pulse jet method and NaOH etching, which has a higher specific surface area, pore volume and more surface alkaline adsorption sites; (2) Before preparing the modified basalt@UiO-66 composite material, the K2O-modified basalt nanofiber is first modified with zirconium chloride and amino groups. Amino group modification can increase the alkaline adsorption sites, and Venturi The dust removal method can load zirconium chloride onto the nanofibers in a highly dispersed manner; (3) The nanofibers loaded with zirconium chloride on the surface react with the synthetic raw materials of UiO-66 to uniformly embed the nanofibers into UiO-66, thereby preparing a modified basalt@UiO-66 composite material with high specific surface area, pore volume and active adsorption sites, thereby having high CO2 adsorption capacity and CO2 / N2 selectivity; (4) The price of the raw material of modified basalt is much lower than that of UiO-66, so the cost of the composite material is reduced, which provides a guarantee for large-scale industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 The SEM images of different samples in the embodiments and comparative examples of the present invention are as follows: (a) CBF MNa , (b) CBF CP , (c) K2O / CBF MNa , (d) UiO-66, (e) K2O / CBF MNa 0.3@UiO-66 1T , (f) K2O / CBF MNa 0.3@UiO-66 2T .
[0027] Figure 2 The CO2 adsorption performance of different samples in the embodiments and comparative examples of the present invention at 150°C is shown as follows: (a) UiO-66, (b) CBF MNa , (c) CBF CP , (d) K2O / CBF MNa , (e) K2O / CBF MNa 0.2@UiO-66 1T , (f) K2O / CBFMNa0.3@UiO-66 1T , (g) K2O / CBFMNa 0.4@UiO-66 1T , (h)K2O / CBF MNa 0.3@UiO-66 2T .
[0028] Figure 3 The adsorption selectivity of different samples for CO2 / N2 in the embodiments and comparative examples of the present invention: (a) UiO-66, (b) CBF MNa , (c) CBF CP , (d) K2O / CBF MNa , (e) K2O / CBF MNa 0.2@UiO-66 1T , (f) K2O / CBF MNa 0.3@UiO-66 1T , (g) K2O / CBF MNa 0.4@UiO-66 1T , (h)K2O / CBF MNa 0.3@UiO-66 2T . DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with specific embodiments and comparative examples. According to the following examples, the present invention can be better understood. However, it is easy for those skilled in the art to understand that the specific material proportions, process conditions and results described in the embodiments are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims.
[0030] Example 1
[0031] (1) basalt is fully ground in a corundum crucible, and then the mixture is melted at 1500° C. to obtain molten basalt. A porous anodic aluminum oxide (AAO) is used as a template, and a pulse jet method is used to spray the molten basalt into the alumina template through compressed air at a pressure of 10 atm, thereby forming nanofibers with rough surfaces in the template;
[0032] (2) Etching with 10 wt% NaOH solution for 1 h to remove the alumina template and components such as silicon oxide and aluminum oxide in basalt, and to strengthen the surface alkalinity of the nanofibers to prepare basalt nanofibers with nanopores, denoted as CBF MNa ;
[0033] Example 2
[0034] (1) basalt is fully ground in a corundum crucible, potassium nitrate is added in a mass ratio of K element to basalt of 1:4, and then the mixture is melted at 1500°C to obtain K2O-modified molten basalt, and porous anodic aluminum oxide (AAO) is used as a template. The K2O-modified molten basalt is sprayed into the alumina template by a pulse jet method through compressed air at a pressure of 10 atm, thereby forming nanofibers with rough surfaces in the template;
[0035] (2) Etching with 10 wt% NaOH solution for 1 h to remove the alumina template and components such as silicon oxide and aluminum oxide in basalt, and to strengthen the surface alkalinity of the nanofibers, thereby preparing K2O-modified basalt nanofibers with nanopores, recorded as K2O / CBF MNa .
[0036] Example 3
[0037] (1) Zirconium chloride was impregnated into K2O-modified basalt nanofibers (K2O / CBF) using the Venturi dust removal method. MNa The specific operation is as follows: the modified basalt nanofibers are placed in the feed hopper of the Venturi dust collector. After the nanofibers are fed, they are dispersed and accelerated by a 40 m / s high-speed airflow in the air inlet pipe, and then enter the throat along the contraction pipe. The diameter ratio of the throat to the air inlet pipe is 1:2. According to the feed mass ratio of zirconium chloride to nanofibers of 3:8, the zirconium chloride solution is sprayed from the nozzles distributed in an annular manner around the throat, and is atomized and accelerated by the high-speed airflow, so that the zirconium chloride droplets fully collide and impregnate the nanofibers, and then enter the cyclone separator along the diffusion pipe and the connecting pipe to complete the gas-solid separation.
[0038] (2) drying the separated solid at 120° C. overnight, then introducing a mixed atmosphere of ammonia:nitrogen=1:9 into a tube furnace, and treating at a high temperature of 400° C. for 4 h to obtain zirconium chloride and amino-modified K2O-modified basalt nanofibers;
[0039] (3) The modified basalt nanofibers, zirconium chloride and terephthalic acid (H2BDC) were dissolved in 130 mL DMF solvent at a mass ratio of 0.2:1.4:1, transferred to a reactor, and reacted at 150 °C for 24 h. After cooling, the precipitate was washed three times with DMF and ethanol, and dried at 160 °C to obtain a modified basalt@UiO-66 composite material, recorded as K2O / CBF MNa 0.2@UiO-66 1T .
[0040] Example 4
[0041] (1) Zirconium chloride was impregnated into K2O-modified basalt nanofibers (K2O / CBF) using the Venturi dust removal method. MNaThe specific operation is as follows: the modified basalt nanofibers are placed in the feed hopper of the Venturi dust collector. After the nanofibers are fed, they are dispersed and accelerated by a 40 m / s high-speed airflow in the air inlet pipe, and then enter the throat along the contraction pipe. The diameter ratio of the throat to the air inlet pipe is 1:2. According to the feed mass ratio of zirconium chloride to nanofibers of 3:8, the zirconium chloride solution is sprayed from the nozzles distributed in an annular manner around the throat, and is atomized and accelerated by the high-speed airflow, so that the zirconium chloride droplets fully collide and impregnate the nanofibers, and then enter the cyclone separator along the diffusion pipe and the connecting pipe to complete the gas-solid separation.
[0042] (2) drying the separated solid at 120° C. overnight, then introducing a mixed atmosphere of ammonia:nitrogen=1:9 into a tube furnace, and treating at a high temperature of 400° C. for 4 h to obtain zirconium chloride and amino-modified K2O-modified basalt nanofibers;
[0043] (3) The modified basalt nanofibers, zirconium chloride and terephthalic acid (H2BDC) were dissolved in 130 mL DMF solvent at a mass ratio of 0.3:1.4:1, transferred to a reactor, and reacted at 150 °C for 24 h. After cooling, the precipitate was washed three times with DMF and ethanol, and dried at 160 °C to obtain a modified basalt@UiO-66 composite material, recorded as K2O / CBF MNa 0.3@UiO-66 1T .
[0044] Example 5
[0045] (1) Zirconium chloride was impregnated into K2O-modified basalt nanofibers (K2O / CBF) using the Venturi dust removal method. MNa The specific operation is as follows: the modified basalt nanofibers are placed in the feed hopper of the Venturi dust collector. After the nanofibers are fed, they are dispersed and accelerated by a 40 m / s high-speed airflow in the air inlet pipe, and then enter the throat along the contraction pipe. The diameter ratio of the throat to the air inlet pipe is 1:2. According to the feed mass ratio of zirconium chloride to nanofibers of 3:8, the zirconium chloride solution is sprayed from the nozzles distributed in an annular manner around the throat, and is atomized and accelerated by the high-speed airflow, so that the zirconium chloride droplets fully collide and impregnate the nanofibers, and then enter the cyclone separator along the diffusion pipe and the connecting pipe to complete the gas-solid separation.
[0046] (2) drying the separated solid at 120° C. overnight, then introducing a mixed atmosphere of ammonia:nitrogen=1:9 into a tube furnace, and treating at a high temperature of 400° C. for 4 h to obtain zirconium chloride and amino-modified K2O-modified basalt nanofibers;
[0047] (3) The modified basalt nanofibers, zirconium chloride and terephthalic acid (H2BDC) were dissolved in 130 mL DMF solvent at a mass ratio of 0.4:1.4:1, transferred to a reactor, and reacted at 150 °C for 24 h. After cooling, the precipitate was washed three times with DMF and ethanol, and dried at 160 °C to obtain a modified basalt@UiO-66 composite material, recorded as K2O / CBF MNa 0.4@UiO-66 1T .
[0048] Comparative Example 1
[0049] Zirconium chloride and terephthalic acid (H2BDC) were dissolved in 130 mL DMF solvent at a mass ratio of 1.4:1, transferred to a reactor, and reacted at 150°C for 24 hours. After cooling, the precipitate was washed three times with DMF and ethanol, and dried at 160°C. The obtained material was recorded as UiO-66.
[0050] Comparative Example 2
[0051] (1) basalt is fully ground in a corundum crucible, and then the mixture is melted at 1500° C. to obtain molten basalt, and porous anodic aluminum oxide (AAO) is used as a template, and the molten basalt is injected into the alumina template by suction filtration to form nanofibers in the template;
[0052] (2) Etching with 10 wt % phosphoric acid solution for 1 h to remove the aluminum oxide template and components such as calcium oxide and magnesium oxide in basalt, weaken the surface alkalinity of the nanofibers, and prepare basalt nanofibers with nanopores, recorded as CBF CP ;
[0053] Comparative Example 3
[0054] K2O modified basalt nanofibers K2O / CBF MNa The mixture was dissolved in 130 mL DMF solvent with zirconium chloride and terephthalic acid (H2BDC) in a mass ratio of 0.3:1.4:1, transferred to a reactor, and reacted at 150 °C for 24 h. After cooling, the precipitate was washed with DMF and ethanol three times and dried at 160 °C to obtain a modified basalt@UiO-66 composite material, recorded as K2O / CBF MNa 0.3@UiO-66 2T .
[0055] The morphology of the samples was tested by SEM, the specific surface area and pore volume of the samples were tested by low-temperature nitrogen physical adsorption, and the CO2 adsorption performance of the materials was investigated by thermogravimetric analyzer. The materials were weighed and loaded into the crucible of a thermobalance, and the temperature was raised to 150°C in a CO2 atmosphere. After keeping warm for 30 minutes, the thermogravimetric curve no longer rose, and the CO2 adsorption capacity of the material at 150°C was measured. The atmosphere was switched to N2, and the N2 adsorption capacity was tested at the same temperature, and then the adsorption selectivity of the material for CO2 / N2 was obtained.
[0056] Depend on Figure 1 (a) shows basalt nanofiber CBF prepared by pulse jet method and NaOH etching. MNa It is in bundle shape, with a length of several hundred nanometers and a diameter of about 30-50nm, accompanied by agglomeration. Figure 1 (b) shows the basalt nanofiber CBF prepared by filtration and phosphoric acid solution etching. CP It is irregularly dispersed, with a length of several hundred nanometers and a diameter of about 30-50nm; Figure 1 (c) shows K2O-doped basalt nanofibers K2O / CBF MNa The diameter of is about 20nm, which is significantly smaller than the first two and has good dispersion. Figure 1 (d) It can be seen that UiO-66 has an octahedral structure with a size of about 10 μm. The octahedral surface is relatively smooth and has some small particles attached to it. Figure 1 (e) It can be seen that K2O / CBF MNa 0.3@UiO-66 1T The octahedral morphology and size of UiO-66 are basically retained, and rough stripes appear on the surface, indicating that the basalt nanofibers and UiO-66 are well composited; Figure 1 (f) It can be seen that K2O / CBF MNa 0.3@UiO-66 2T There are both rough-surfaced octahedrons and independent bundles of fibers, indicating that the composite of basalt nanofibers and UiO-66 is poor.
[0057] As shown in Table 1, the specific surface area and pore volume of UiO-66 are 812 m 2 / g and 0.65m 3 / g. Basalt nanofiber CBF MNa The specific surface area and pore volume are 231m 2 / g and 0.36m 3 / g. In comparison, K2O / CBF MNa The specific surface area and pore volume are 218m 2 / g and 0.35m 3 / g, only a slight decrease was observed; while CBFCP The specific surface area and pore volume are 176m 2 / g and 0.29m 3 / g, the decrease is obvious. K2O / CBF MNa The specific surface area and pore volume of the composite material with UiO-66 first increased and then decreased with the increase of basalt nanofiber doping amount. MNa 0.3@UiO-66 1T The highest specific surface area and pore volume were obtained, which were 1023m 2 / g and 0.76m 3 / g. In contrast, K2O / CBF MNa 0.3@UiO-66 2T The specific surface area and pore volume are 917m 2 / g and 0.71m 3 / g, which is due to K2O / CBF MNa It is caused by poor compounding with UiO-66.
[0058] Table 1 Specific surface area and pore volume test results of samples
[0059]
[0060]
[0061] Figure 2 The CO2 adsorption capacity of the products obtained from different embodiments and comparative examples at 150°C. The CO2 adsorption capacity of the UiO-66 matrix is 1.42 mmol / g. MNa and CBF CP The CO2 adsorption capacity of CBF is 0.34mmol / g and 0.21mmol / g respectively. The former is higher than the latter. MNa The NaOH etching solution used in the preparation can increase the surface alkaline sites of the nanofibers, while the CBF CP The phosphoric acid etching solution used in the preparation will reduce the surface alkaline sites of the nanofibers; MNa Compared with K2O / CBF MNa The CO2 adsorption capacity of K2O / CBF increased to 0.41mmol / g, which is due to the fact that K2O provides more adsorption sites. MNa The CO2 adsorption capacity of the composite material with UiO-66 first increased and then decreased with the increase of basalt nanofiber doping amount. MNa 0.3@UiO-66 1T The highest CO2 adsorption capacity was 4.28mmol / g. MNa 0.3@UiO-662T The CO2 adsorption capacity is only 3.24mmol / g, and the law of CO2 adsorption capacity is basically consistent with the law of specific surface area.
[0062] Figure 3 is the adsorption selectivity of the sample for CO2 / N2. The adsorption selectivity of UiO-66 matrix for CO2 / N2 is 13.7. MNa and CBF CP The selectivities of CBF are 21.6 and 12.8, respectively. The former is higher than the latter because the former has more surface basic sites. MNa Compared with K2O / CBF MNa The selectivity for CO2 / N2 increased to 29.4, which is due to the fact that K2O provides more chemical adsorption sites. K2O / CBF MNa The selectivity of K2O / CBF composites to CO2 / N2 first increases and then decreases with the increase of basalt nanofiber doping amount. MNa 0.3@UiO-66 1T The highest selectivity was 27.2. In comparison, K2O / CBF MNa 0.3@UiO-66 2T The selectivity for CO2 / N2 is only 23.2.
[0063] Table 2 pH values of samples when zeta potential is zero before and after CO2 adsorption
[0064]
[0065]
[0066] The pH value (pH) when the zeta potential of the sample is zero before and after CO2 adsorption pzc ) As shown in Table 2, before CO2 adsorption, the pH of UiO-66 pzc is 7.3, close to neutral; CBF MNa CBF CP and K2O / CBF MNa pH pzc The values were 11.5, 7.9 and 11.7 respectively. After compounding with UiO-66, the pH value of the material pzc Range is 9.5-10.9, K2O / CBF MNa 0.3@UiO-66 1T Get the highest pH pzc Value, specific surface area, pore volume and pH pzc The values jointly determine the material's highest CO2 adsorption capacity and selectivity.
Claims
1. A modified basalt@UiO-66 composite material, It is characterized in that Modified basalt to K 2 O-modified basalt nanofibers have a diameter of 15-25 nm, the mass ratio of K element to basalt in the modified basalt is 1:4, and the mass ratio of modified basalt to UiO-66 is (0.2-0.4):1.
6.
2. The modified basalt@UiO-66 composite material according to claim 1, It is characterized in that The specific surface area of the modified basalt@UiO-66 composite material is 936-1023m 2 / g, pore volume is 0.72-0.76m 3 / g.
3. The modified basalt@UiO-66 composite material according to claim 1, It is characterized in that The preparation method of the modified basalt is as follows: Step 1: Grind basalt in a corundum crucible, add potassium nitrate, and then melt the mixture at the melting temperature to obtain K 2 O-modified molten basalt was used as a template for K-ionization by pulse jet method. 2 O-modified molten basalt is sprayed into the alumina template to form nanofibers with rough surface in the alumina template; Step 2: Use a certain concentration of NaOH solution to etch away the alumina template and the silicon oxide, aluminum oxide and other components in the basalt, and strengthen the surface alkalinity of the nanofibers to prepare K nanofibers with nanopores. 2 O modified basalt nanofibers.
4. A method for preparing the modified basalt@UiO-66 composite material as claimed in claim 1, It is characterized in that The following steps are involved: Step 1: Grind basalt in a corundum crucible, add potassium nitrate, and then melt the mixture at the melting temperature to obtain K 2 O-modified molten basalt was used as a template for K-ionization by pulse jet method. 2 O-modified molten basalt is sprayed into the alumina template to form nanofibers with rough surface in the alumina template; Step 2: Use a certain concentration of NaOH solution to etch away the alumina template and the silicon oxide, aluminum oxide and other components in the basalt, and strengthen the surface alkalinity of the nanofibers to prepare K nanofibers with nanopores. 2 O modified basalt nanofibers; Step 3, using the Venturi dust removal method to impregnate zirconium chloride into the K prepared in step 2 2 In the basalt nanofibers modified with K 2 O modified basalt nanofibers are placed in the feed hopper of the venturi dust collector, K 2 After the O-modified basalt nanofibers are fed, they are dispersed and accelerated by the high-speed airflow in the air inlet pipe, and then enter the throat along the contraction tube. The zirconium chloride solution is sprayed out from the nozzles distributed in an annular manner around the throat, and is atomized and accelerated by the high-speed airflow, completing the zirconium chloride droplet to K 2 The O-modified basalt nanofibers fully collide and impregnate, and then enter the cyclone separator along the diffusion pipe and the connecting pipe to complete the gas-solid separation; Step 4, drying the solid separated in step 3, and then treating it at high temperature in a tube furnace for 4 hours to obtain zirconium chloride and amino-modified K 2 O modified basalt nanofibers; Step 5, the zirconium chloride prepared in step 4 and amino-modified K 2 UiO-66 modified basalt nanofibers, zirconium chloride and terephthalic acid were dissolved in DMF solvent in a certain mass ratio, transferred to a reactor, and reacted at 150°C for 24 hours. After cooling, the precipitate was washed three times with DMF and ethanol, and dried at 160°C to obtain the final modified basalt@UiO-66 composite material.
5. The method for preparing the modified basalt@UiO-66 composite material according to claim 4, It is characterized in that In step 1, the mass ratio of K element in potassium nitrate to basalt is 1:4, the melting temperature is 1500°C, and the pulse jet method is to mix 1500°C compressed air and K 2 The O-doped molten basalt mixed injection method uses a compressed air pressure of 10 atm.
6. The method for preparing the modified basalt@UiO-66 composite material according to claim 4, It is characterized in that In step 2, the concentration of NaOH solution is 10wt%, and the treatment time is 1h.
7. The method for preparing the modified basalt@UiO-66 composite material according to claim 2, It is characterized in that The velocity of the high-speed airflow in the inlet pipe in step 3 is 40 m / s, the diameter ratio of the throat pipe to the inlet pipe is 1:2, and the ratio of zirconium chloride to K 2 The feed mass ratio of O-modified basalt nanofibers was 3:
8.
8. The method for preparing the modified basalt@UiO-66 composite material according to claim 4, It is characterized in that The drying temperature in step 4 is 120° C., the temperature of the high temperature treatment in the tube furnace is 400° C., and the atmosphere is a mixed atmosphere of ammonia:nitrogen=1:
9.
9. The method for preparing the modified basalt@UiO-66 composite material according to claim 4, It is characterized in that In step 5, zirconium chloride and amino-modified K 2 The mass ratio of O-modified basalt nanofibers to zirconium chloride and terephthalic acid is (0.2-0.4):1.4:
1.
10. An application of the modified basalt@UiO-66 composite material as claimed in any one of claims 1 to 3 for CO 2 adsorption.
Citation Information
Cited By
Modified heavy-load asphalt mixture based on basalt fiber composite material as well as preparation method and application of modified heavy-load asphalt mixture
CN120271274A