Method for preparing lithium carbonate from lepidolite
Through the sulfuric acid pressure cooking method and multi-step crystallization process, the problem of high energy consumption and resource waste in the process of extracting lithium from lepidolite is solved, efficient and low-energy utilization of lepidolite resources is realized, and white lithium slag suitable for building materials and ceramics is generated. , improving the comprehensive utilization value of lepidolite.
Patent Information
- Application Number
- CN202410838607.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
AI Technical Summary
Existing methods for extracting lithium from lepidolite, such as sulfate roasting, require high temperatures, resulting in high energy consumption and the production of unused valuable metals and impurity slag, which reduces resource utilization and environmental impact.
Lepidolite is finely ground and pressure-leached at low temperature using the sulfuric acid pressure cooking method, and lithium is extracted through a multi-step freezing crystallization, thermal crystallization and extraction process, combined with potassium fluoride and ammonia water treatment, to achieve efficient extraction of lithium and comprehensive utilization of valuable resources. , producing white low-toxic residue.
It achieves high leaching rate and low energy consumption of lithium in lepidolite, reduces the amount of slag, improves the comprehensive utilization value and product purity of lepidolite, and is suitable for the building materials and ceramic industries.
Smart Images

Figure CN118724029A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium carbonate preparation, in particular to a method for preparing lithium carbonate from lepidolite. Background Art
[0002] Lepidolite is a lithium-rich mineral resource with wide application value in multiple industrial fields. In particular, Yichun, Jiangxi Province, China has rich lepidolite mineral resources, which contain not only lithium, but also expensive rubidium and cesium elements and a large amount of valuable resources such as aluminum, potassium and fluorine. How to extract these valuable elements efficiently and environmentally friendly, and convert the remaining slag into valuable raw materials such as chemicals, ceramics, and building materials, is of great significance to improving the comprehensive utilization value of lepidolite.
[0003] At present, the lithium extraction industry mainly uses sulfate roasting method. Although this method can achieve lithium extraction to a certain extent, it has the following disadvantages: The sulfate roasting method requires a high temperature environment for reaction, which leads to high energy consumption and increased production costs. At the same time, the slag produced after sulfate roasting contains unextracted valuable metals and other components. Since it is difficult to further process, it is often treated as waste, which not only wastes resources, but also increases the environmental burden and reduces the comprehensive utilization value of lithium mica. Summary of the invention
[0004] The invention aims to provide a method for preparing lithium carbonate from lepidolite. The method for preparing lithium carbonate from lepidolite adopts a sulfuric acid pressure boiling method to extract lithium from the lepidolite, which can not only achieve low energy consumption and high lithium yield, but also comprehensively utilize other valuable resources in the lepidolite. Meanwhile, the precipitated lithium slag is white and has a small slag amount, and can be widely used in the building materials and ceramic industries, thereby improving the comprehensive utilization value of the lepidolite.
[0005] The above-mentioned optimized structure of the present invention is achieved by the following technical scheme: A method for preparing lithium carbonate from lepidolite comprises the following steps: Step 1: finely grind the dry lithium mica concentrate, and use sulfuric acid to perform pressure leaching within a certain temperature range, and then filter to remove solid impurities to obtain a leachate and lithium slag; Step 2: deacidifying the leaching solution to obtain a deacidified solution; Step 3: subjecting the deacidified liquid to a first freezing treatment to allow it to undergo cooling crystallization, and subjecting it to centrifugal separation to obtain a first crystal and a first separated liquid; Step 4: adding potassium fluoride to the first separated liquid, controlling the molar ratio of fluoride and aluminum ions in the solution to perform a heating reaction, maintaining a preset heating reaction time, and generating a second crystal and a precipitate by thermal crystallization; Step 5: After the precipitate is evaporated and concentrated by 1 to 1.5 times, it is frozen for the second time to cause cooling crystallization, and centrifuged to obtain a third crystal and a second separated liquid; Step 6: extracting and stripping the second separated liquid using an extractant to further purify the second separated liquid to obtain a stripping liquid and a raffinate; Step 7: The stripping solution is subjected to lithium precipitation processing to obtain lithium carbonate, and the raffinate is evaporated to obtain ammonium sulfate.
[0006] In this embodiment, the concentration of sulfuric acid in step 1 is 30%-50%, and the temperature is controlled at 150°C-180°C.
[0007] In this embodiment, in step 2, the acid removal treatment is to add ammonia water to the leachate.
[0008] In this embodiment, in step 3, the temperature of the cooling crystallization is maintained at 0°C-10°C.
[0009] In this embodiment, the first crystal is ammonium alum.
[0010] In this embodiment, in step 4, the molar ratio of fluorinated aluminum ions in the solution is 4:1 to 6:1, the heating temperature is controlled at 75-90° C., and the preset heating reaction time is 30-50 minutes.
[0011] In this embodiment, the third crystal is a mixture of ferric ammonium alum and manganese ammonium alum.
[0012] In this embodiment, in step 5, the evaporation rate of the precipitate is controlled at 5%-10% of the total volume of the evaporating solution per hour, and the temperature of the cooling crystallization is maintained at 0°C-10°C to ensure the yield and purity of the third crystals.
[0013] In this embodiment, in step 6, the extractant is trioctylphosphine oxide.
[0014] In this embodiment, in step 6, the extraction and stripping are multi-stage countercurrent extraction processes.
[0015] One or more of the above technical solutions in the embodiments of the present invention have at least the following technical effects or advantages: (1) High leaching rate and low energy consumption: The leaching rate of lithium oxide in lepidolite by the method of the present invention is as high as 99.93%, which is much higher than the traditional sulfate roasting method. At the same time, the full wet sulfuric acid pressure cooking method significantly reduces energy consumption compared with the roasting method, thereby improving the economic benefits of lithium extraction from lepidolite.
[0016] (2) Comprehensive utilization of valuable resources: The method of the present invention can not only extract lithium from lithium mica, but also leaching out valuable metal ions such as potassium, rubidium, cesium, and aluminum. Through specific process steps, these resources can be effectively separated and recovered, realizing the comprehensive utilization of valuable resources and improving the comprehensive utilization value of lithium mica.
[0017] (3) Reducing the amount of slag and improving the slag quality: The lithium slag produced by the method of the present invention is white, the amount of slag is small, and all toxic substances are leached out, resulting in low toxicity. It has a wide range of uses in the building materials and ceramic industries and can effectively solve the problem of lithium slag retention in the industry.
[0018] (4) Impurity removal and product purity improvement: Through a two-step cold crystallization and one-step hot crystallization process, the present invention effectively removes impurity ions in brine, such as aluminum, fluorine, iron, manganese, etc., and improves the purity of the final product lithium carbonate; at the same time, these crystallized salts can be used as by-products, further reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 The present invention is a schematic flow chart of the method for preparing lithium carbonate from lepidolite. DETAILED DESCRIPTION
[0021] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0022] In the description of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0023] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0024] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0025] refer to Figure 1 , a method for preparing lithium carbonate from lepidolite, comprising the following steps: Step 1: Grind the dry lithium mica concentrate to obtain lithium mica with a particle size range of 150-200 mesh; and use sulfuric acid with a concentration of 30%-50% to perform pressure leaching at a temperature range of 150°C-180°C, and then filter to remove solid impurities to obtain a leachate and lithium slag; Step 2: adding ammonia water to the leaching solution for deacidification to obtain a deacidified solution; Step 3: subjecting the deacidified liquid to a first freezing treatment, cooling and crystallizing it at a temperature of 0°C-10°C, and obtaining a first crystal (ammonium alum) and a first separated liquid by centrifugation; Step 4: adding potassium fluoride to the first separated liquid, controlling the molar ratio of fluoride and aluminum ions in the solution to be 4:1 to 6:1, heating the reaction at a temperature of 75-90°C for 30-50 minutes, and generating a second crystal and a precipitate by thermal crystallization. The second crystal is potassium cryolite (potassium hexafluoroaluminate), which can effectively remove aluminum and fluoride ions in brine; Step 5: After the precipitate is evaporated and concentrated by 1 to 1.5 times, it is frozen again, cooled and crystallized at a temperature of 0°C-10°C, and centrifuged to obtain a third crystal (a mixture of ammonium ferric alum and ammonium manganese alum) and a second separated liquid, which can effectively remove metal impurity ions such as iron and manganese in the precipitate; the evaporation rate is controlled at 5%-10% of the total volume of the evaporated solution per hour to ensure the yield and purity of ammonium ferric alum and ammonium manganese alum; Step 6: using an alkaline lithium ion extractant such as trioctylphosphine oxide (TOPO) as an extractant, the second separated liquid is subjected to multi-stage countercurrent extraction and stripping operations for further purification to obtain a stripping solution and a raffinate, wherein the stripping solution may be a lithium-rich solution, and the raffinate may be a high-purity, high-solubility ammonium sulfate solution; Step 7: obtain lithium carbonate by adding soda ash or introducing CO2, and evaporate the raffinate to obtain ammonium sulfate.
[0026] Embodiment 1: The 150 mesh lithium mica concentrate was pressure-leached at 180°C using a 40% sulfuric acid solution, and the remaining steps were performed according to the above method.
[0027] In step 3, the crystallization temperature of the acid removal solution is controlled at 0°.
[0028] In step 4, the molar ratio of fluorine aluminum ions in the solution is controlled to be 5:1, the heating temperature is 80° C., and the heating reaction time is 40 minutes.
[0029] In step 5, the evaporation concentration multiple of the precipitate is 1.2 times, the crystallization temperature is controlled at 0°, and the evaporation rate is 7% of the total volume of the evaporated solution per hour.
[0030] In step 6, a two-stage countercurrent extraction process is used for extraction and stripping. The lithium content of the stripping solution reaches more than 40 g / L, providing a high-concentration raw material for subsequent lithium precipitation processing.
[0031] In step 7, sodium carbonate is used as a precipitant in lithium precipitation processing, and the reaction conditions are normal temperature and pressure. The final lithium carbonate product obtained has high purity and uniform particle size, meeting market requirements. The final lithium carbonate yield is 95%, the purity of lithium carbonate reaches 99.5%, and the recovery rates of aluminum, potassium, and fluorine all reach more than 90%.
[0032] Example 2 The 180 mesh lithium mica concentrate was pressure leached at 150°C using a 45% sulfuric acid solution.
[0033] The crystallization temperature of the acid-removing liquid is controlled at 5° C., and the first crystals and the first separated liquid are obtained by centrifugal separation.
[0034] The molar ratio of fluoride and aluminum ions in the solution was controlled to be 5.5:1, the heating temperature was 85° C., and the heating reaction time was 42 minutes.
[0035] The evaporation concentration multiple of the precipitate is 1.3 times, the crystallization temperature is controlled at 3°C, and the evaporation rate is 8% of the total volume of the evaporated solution per hour.
[0036] A two-stage countercurrent extraction process was used for extraction and stripping. The lithium content of the stripping solution reached 45g / L.
[0037] Sodium carbonate is used as the precipitant in the lithium precipitation process. The final lithium carbonate yield is 95.5%, the purity reaches 97.6%, and the recovery rates of aluminum, potassium and fluorine are all over 91%.
[0038] Example 3 The 200-mesh lithium mica concentrate was pressure-leached at 180°C using a 35% sulfuric acid solution.
[0039] The crystallization temperature of the acid removal solution is controlled at 8°C.
[0040] The molar ratio of fluoride and aluminum ions in the solution was controlled to be 4.5:1, the heating temperature was 78° C., and the heating reaction time was 39 minutes.
[0041] The evaporation concentration multiple of the precipitate was 1.1 times, the crystallization temperature was controlled at 6°C, and the evaporation rate was 6% of the total volume of the evaporated solution per hour.
[0042] The extraction and stripping operations were carried out using a two-stage countercurrent extraction process. The lithium content of the stripping solution reached 35g / L.
[0043] The lithium precipitation process uses a combination of sodium carbonate and CO2 injection. The final lithium carbonate yield is 94.8%, the purity reaches 99.4%, and the recovery rates of aluminum, potassium and fluorine are all over 90%.
[0044] Example 4 The 200-mesh lithium mica concentrate was pressure-leached at 180°C using 50% sulfuric acid.
[0045] The crystallization temperature of the acid removal solution is controlled at 10°C.
[0046] The molar ratio of fluorine and aluminum ions in the solution was controlled to be 6:1, the heating temperature was 90° C., and the heating reaction time was 45 minutes.
[0047] The evaporation concentration multiple of the precipitate was 1.4 times, the crystallization temperature was controlled at 8°C, and the evaporation rate was 9% of the total volume of the evaporated solution per hour.
[0048] The extraction and stripping operations were carried out using a two-stage countercurrent extraction process. The lithium content of the stripping solution reached 60g / L.
[0049] The lithium precipitation process only uses the method of introducing CO2, and the final lithium carbonate yield is 96.2%, the purity reaches 99.7%, and the recovery rates of aluminum, potassium and fluorine are all over 92%.
[0050] Example 5 The 160 mesh lithium mica concentrate was pressure leached at 180°C using a 30% sulfuric acid solution.
[0051] The crystallization temperature of the acid removal solution is controlled at 1°C.
[0052] The molar ratio of fluoride and aluminum ions in the solution was controlled to be 4.2:1, the heating temperature was 75° C., and the heating reaction time was 38 minutes.
[0053] The evaporation concentration multiple of the precipitate is 1, the crystallization temperature is controlled at 1°C, and the evaporation rate is 5% of the total volume of the evaporated solution per hour.
[0054] The three-stage countercurrent extraction process is used for extraction and stripping. The lithium content of the stripping solution reaches 30g / L.
[0055] The lithium precipitation process uses sodium carbonate as a precipitant and is assisted by the introduction of CO2. The final lithium carbonate yield is 94.5%, the purity reaches 99.3%, and the recovery rates of aluminum, potassium, and fluorine are all over 89%.
[0056] In summary, the present invention provides a method for preparing lithium carbonate by efficient and comprehensive utilization of lepidolite. The method uses sulfuric acid to pressure-leach finely ground lepidolite concentrate to leach valuable metal ions such as potassium, rubidium, cesium, aluminum and toxic substances in the lepidolite concentrate, thereby obtaining white non-toxic lithium slag, which meets the application requirements of the building materials and ceramic industries, effectively solves the problem of lithium slag retention, and effectively removes impurity ions in brine through a process of deacidification with ammonia water, adding potassium fluoride, adopting two-step cold crystallization and one-step hot crystallization, thereby improving the purity of the final product lithium carbonate; and precipitating these impurity ions in the form of crystalline salts, which can be used as by-products, further reducing the production cost; thereby achieving high yield and high purity of lithium carbonate.
[0057] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing lithium carbonate from lepidolite, characterized in that: The following steps are involved: Step 1: finely grind the dry lithium mica concentrate, and use sulfuric acid to perform pressure leaching within a certain temperature range, and then filter to remove solid impurities to obtain a leachate and lithium slag; Step 2: deacidifying the leaching solution to obtain a deacidified solution; Step 3: subjecting the deacidified liquid to a first freezing treatment to allow it to undergo cooling crystallization, and subjecting it to centrifugal separation to obtain a first crystal and a first separated liquid; Step 4: adding potassium fluoride to the first separated liquid, controlling the molar ratio of fluoride and aluminum ions in the solution to perform a heating reaction, maintaining a preset heating reaction time, and generating a second crystal and a precipitate by thermal crystallization; Step 5: After the precipitate is evaporated and concentrated by 1 to 1.5 times, it is subjected to a second freezing treatment to allow cooling and crystallization to occur, and centrifuged to obtain a third crystal and a second separated liquid; Step 6: extracting and stripping the second separated liquid using an extractant to further purify the separated liquid to obtain a stripping liquid and a raffinate; Step 7: The stripping solution is subjected to lithium precipitation processing to obtain lithium carbonate, and the raffinate is evaporated to obtain ammonium sulfate.
2. A method for preparing lithium carbonate from lepidolite according to claim 1, characterized in that: The concentration of sulfuric acid in step 1 is 30%-50%, and the temperature is controlled at 150°C-180°C.
3. A method for preparing lithium carbonate from lepidolite according to claim 1, characterized in that: In the step 2, the deacidification treatment is to add ammonia water to the leachate.
4. The method for preparing lithium carbonate from lepidolite according to claim 1, wherein: In the step 3, the temperature of the cooling crystallization is maintained at 0°C-10°C.
5. A method for preparing lithium carbonate from lepidolite according to claim 4, characterized in that, The first crystal is ammonium alum.
6. The method for preparing lithium carbonate from lepidolite according to claim 1, wherein: In step 4, the molar ratio of fluoride aluminum ions in the solution is 4:1 to 6:1, the heating temperature is controlled at 75-90° C., and the preset heating reaction time is 30-50 minutes.
7. The method for preparing lithium carbonate from lepidolite according to claim 1, wherein: The third crystal is a mixture of ferric ammonium alum and manganese ammonium alum.
8. The method for preparing lithium carbonate from lepidolite according to claim 1, wherein: In the step 5, the evaporation rate of the precipitate is controlled at 5%-10% of the total volume of the evaporating solution per hour, and the temperature of the cooling crystallization is maintained at 0°C-10°C to ensure the yield and purity of the third crystal.
9. The method for preparing lithium carbonate from lepidolite according to claim 1, wherein: In step 6, the extractant is trioctylphosphine oxide.
10. The method for preparing lithium carbonate from lepidolite according to claim 1, characterized in that: In step 6, the extraction and stripping are multi-stage countercurrent extraction processes.
Citation Information
Cited By
Method for preparing battery grade lithium carbonate by utilizing battery material raffinate
CN121317828A