Method for preparing porous FeS2 (at) C nano-particles by using retired lithium iron phosphate battery positive electrode material, FeS2 (at) C nano-particles and application of FeS2 (at) C nano-particles

Porous FeS2@C nanoparticles are prepared by recycling retired lithium iron phosphate batteries, which solves the problems of poor conductivity and volume change of potassium-ion battery materials, improves the cycle stability and discharge capacity of potassium-ion batteries, and achieves efficient recycling of retired materials. , has significant economic and social benefits.

CN118724075APending Publication Date: 2024-10-01ALPHA ESS CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410712182.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Due to the large radius of potassium ions in potassium-ion batteries, it becomes more difficult to deintercalate during charging and discharging. Traditional lithium-ion battery materials cannot be directly used in potassium-ion batteries, and the poor conductivity and volume change of the FeS2 anode material limit its practical application.

Method used

By recycling retired lithium iron phosphate battery cathode materials, porous FeS2@C nanoparticles are prepared using traditional hydrothermal methods, and metal organic framework MIL-100(Fe) is used as the FeS2 precursor to provide controllable nanostructure and ordered carbon substrate. , forming a honeycomb porous structure to improve electrical conductivity.

Benefits of technology

It significantly improves the specific discharge capacity and cycle stability of potassium-ion batteries, reduces the volume expansion of potassium-ion batteries during the potassium embedding process, improves cycle performance, and enables efficient recycling of decommissioned materials, which has economic and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724075A_ABST
    Figure CN118724075A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing porous FeS < 2 >-C nano-particles by using a positive electrode material of a decommissioned lithium iron phosphate battery, the FeS < 2 >-C nano-particles and application of the FeS < 2 >-C nano-particles, and the method comprises the following steps: firstly, soaking the decommissioned lithium iron phosphate battery in saline water for discharging, then disassembling, sorting out a positive electrode plate, calcining, separating out lithium iron phosphate positive electrode powder, and drying to obtain the porous FeS < 2 >-C nano-particles; soaking the lithium iron phosphate positive electrode powder in an acid solution, stirring until the lithium iron phosphate positive electrode powder is completely dissolved, centrifuging and filtering to obtain an acid leaching solution, adding an alkali solution while stirring until the pH value is 4-6 to obtain a suspension, sequentially centrifuging, washing and drying to obtain pure ferric hydroxide powder, uniformly mixing the ferric hydroxide powder, 1, 3, 5-benzene tricarbonic acid, water and concentrated nitric acid, and drying to obtain the lithium iron phosphate positive electrode material. The preparation method comprises the following steps: firstly, preparing a porous FeS2atC nano-particle, transferring the porous FeS2atC nano-particle into a polytetrafluoroethylene high-pressure reaction kettle, carrying out hydrothermal reaction, centrifuging, washing and drying to obtain MIL-100 (Fe), finally mixing the MIL-100 (Fe) and sublimed sulfur, filling into a sleeve, and calcining twice in a nitrogen atmosphere to obtain the porous FeS2atC nano-particle which has high conductivity and a porous structure and endows a potassium ion battery with relatively high specific discharge capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of potassium ion batteries, and specifically relates to a method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials, FeS2@C nanoparticles and applications thereof Background Art

[0002] With the vigorous development of the new energy vehicle market in recent years, the power battery market dominated by lithium-ion batteries has ushered in explosive growth. For this reason, more and more retired lithium-ion batteries urgently need to be reasonably and efficiently processed and recycled for reuse, so as to effectively reduce the waste of valuable metal resources and reduce corporate production costs. At the same time, it can also prevent waste power batteries from causing irreversible harm to the environment.

[0003] Potassium has similar chemical properties to lithium. It is abundant in the earth's crust and inexpensive. Therefore, potassium-ion batteries are considered to be energy storage devices that can replace lithium-ion batteries for large-scale applications. However, due to the small radius of potassium ions, Lithium ion radius It is much larger, which increases the difficulty of potassium ion deintercalation during the charging and discharging process, making it impossible to directly use the traditional lithium-ion battery graphite negative electrode on the potassium-ion battery. Therefore, it is very necessary to develop a potassium-ion battery negative electrode material with high specific energy by recycling retired lithium iron phosphate batteries to improve the specific capacity and cycle life of potassium-ion batteries.

[0004] The study found that among the recognized carbonaceous, alloy and conversion-type anode materials, transition metal sulfides (TMSs) have outstanding characteristics such as high theoretical capacity, strong cycle stability and strong redox reversibility. Among the many TMSs materials, FeS2 anode material has a high theoretical capacity (894 mAh g -1 However, its practical application is restricted by many factors, such as poor conductivity, severe volume change, and easy formation of polysulfides during the cycle. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials, FeS2@C nanoparticles and their applications. Using retired waste lithium iron phosphate battery positive electrode materials as raw materials, porous FeS2@C nanoparticles with high conductivity are prepared, which can give potassium ion batteries a higher discharge specific capacity and cycle stability.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials comprises the following steps:

[0008] Step 1: first remove the outer packaging of the retired lithium iron phosphate battery to expose the aluminum shell, and then immerse the retired lithium iron phosphate battery in salt water for discharge;

[0009] Step 2: dismantle the discharged retired lithium iron phosphate battery and sort out the positive electrode sheet;

[0010] Step 3: Place the positive electrode sheet in a muffle furnace for calcination to remove the binder and the current collector aluminum foil on the positive electrode sheet and separate the lithium iron phosphate positive electrode powder;

[0011] Step 4, immerse 1-3 g of lithium iron phosphate positive electrode powder in 15-45 mL of an acidic solution with a concentration of 1 M, stir at 45-70° C. to completely dissolve the lithium iron phosphate, centrifuge and filter to obtain an acid leaching solution containing iron, lithium and phosphate ions;

[0012] Step 5, while stirring the acid leaching solution, add an alkaline solution to the acid leaching solution until the pH value is 4 to 6, to obtain a suspension containing iron hydroxide precipitate;

[0013] Step 6, centrifuging, washing and drying the suspension in sequence to obtain pure ferric hydroxide powder;

[0014] Step 7, according to the molar ratio of ferric hydroxide, 1,3,5-benzenetricarboxylic acid, concentrated nitric acid and water of 1:0.67:166:0.6, ferric hydroxide powder, 1,3,5-benzenetricarboxylic acid, water and concentrated nitric acid with a mass fraction of 65% are mixed and stirred evenly, and after the color changes from reddish brown to orange-yellow, the mixture is transferred to a polytetrafluoroethylene high-pressure reactor, and hydrothermally reacted at 150-180° C. for 10-20 hours, and then centrifuged, washed and dried in sequence to obtain MIL-100(Fe);

[0015] Step 8. Mix and grind MIL-100 (Fe) and commercial sublimed sulfur in a mass ratio of 1: (2-3), put the mixture into a casing, place the casing into a tubular furnace filled with nitrogen, heat the temperature from room temperature to 100-150°C at a heating rate of 5°C / min and keep it warm for 1-2h, then continue to heat the temperature to 400-500°C at a heating rate of 5°C / min and keep it warm for 4-6h. After cooling, porous FeS2@C nanoparticles are obtained.

[0016] Furthermore, the brine in step 1 is a sodium chloride solution with a concentration of 2M.

[0017] Furthermore, the calcination in step 3 is carried out at 400-600° C. and kept warm for 1-3 hours.

[0018] Furthermore, the acidic solution in step 4 is: sulfuric acid, hydrochloric acid or nitric acid solution.

[0019] Furthermore, the stirring in step 4 is carried out at a speed of 200 to 600 r / min for 2 to 4 hours.

[0020] Furthermore, the alkaline solution in step 5 is sodium hydroxide, potassium hydroxide or sodium carbonate solution.

[0021] Furthermore, the stirring in step 5 is carried out at a rotation speed of 200 to 600 r / min.

[0022] Furthermore, the sleeve in step 8 is a quartz sleeve, and the tube mouth of the sleeve faces the nitrogen inlet of the tubular furnace.

[0023] A porous FeS2@C nanoparticle.

[0024] Application of porous FeS2@C nanoparticles as anode materials for potassium-ion batteries.

[0025] Compared with the prior art, the present invention has the following technical effects:

[0026] The present invention uses recycled retired waste lithium iron phosphate battery positive electrode sheets as raw materials, adopts a traditional hydrothermal method to prepare MIL-100 (Fe), and then mixes it with commercial sublimated sulfur and calcines it to obtain porous FeS2@C nanoparticles. The metal organic framework MIL-100 (Fe) serves as a FeS2 precursor to provide a controllable nanostructure and an ordered carbon substrate for FeS2, so that the porous FeS2@C nanoparticles have a honeycomb porous structure and excellent conductive properties. When applied to the negative electrode material of potassium ion batteries, the volume expansion of potassium ion batteries during the potassium insertion process can be effectively reduced, and the cycle performance of potassium ion batteries can be greatly improved, showing a higher discharge specific capacity and cycle stability.

[0027] The present invention can fully recycle and utilize retired waste lithium iron phosphate battery positive electrode plates, reduce the waste of valuable metal resources and the irreversible harm to the environment caused by waste power batteries, and has significant economic and social benefits.

[0028] The preparation process of the invention is simple, the conditions are moderate, and it is safe. The raw materials are cheap and readily available, and the requirements for equipment are low, which is conducive to large-scale batch production. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a process flow chart of the present invention;

[0030] Figure 2 is the X-ray diffraction pattern of MIL-100(Fe) prepared in Example 1 of the present invention;

[0031] Figure 3 is an X-ray diffraction pattern of porous FeS2@C nanoparticles prepared in Example 1 of the present invention;

[0032] Figure 4 is a SEM image of porous FeS2@C nanoparticles prepared in Example 1 of the present invention;

[0033] Figure 5 The cyclic voltammetry curve of the battery when the porous FeS2@C nanoparticles prepared in Example 1 of the present invention are used as the negative electrode material of the potassium ion battery;

[0034] Figure 6 When the porous FeS2@C nanoparticles prepared in Example 1 of the present invention and commercially available FeS2 are used as the negative electrode materials of potassium ion batteries, the battery -1 Cycle diagram under current density. DETAILED DESCRIPTION

[0035] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.

[0036] The process of preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials is as follows: Figure 1 shown.

[0037] Example 1

[0038] Step 1: first remove the outer packaging of the retired lithium iron phosphate battery to expose the aluminum shell, and then immerse the retired lithium iron phosphate battery in a 2M sodium chloride solution and discharge it for 2 days;

[0039] Step 2: dismantle and sort the discharged retired lithium iron phosphate batteries to separate the positive electrode sheets;

[0040] Step 3: Place the positive electrode sheet in a muffle furnace at 400° C. for 3 hours to remove the binder and the current collector aluminum foil on the positive electrode sheet and separate the lithium iron phosphate positive electrode powder;

[0041] Step 4, immerse 1g of lithium iron phosphate positive electrode powder in 15mL of 1M sulfuric acid solution, stir at 45°C and 500r / min for 4h to completely dissolve the lithium iron phosphate, centrifuge and filter to obtain an acid leaching solution containing iron, lithium and phosphate ions;

[0042] Step 5, while stirring the acid leaching solution at a speed of 200 r / min, adding sodium hydroxide solution to the acid leaching solution until the pH value is 4, to obtain a suspension containing iron hydroxide precipitate;

[0043] Step 6, centrifuging, washing and drying the suspension in sequence to obtain pure ferric hydroxide powder;

[0044] Step 7, according to the molar ratio of ferric hydroxide, 1,3,5-benzenetricarboxylic acid, concentrated nitric acid and water of 1:0.67:166:0.6, ferric hydroxide powder, 1,3,5-benzenetricarboxylic acid, water and concentrated nitric acid with a mass fraction of 65% are mixed, stirred at a speed of 300 r / min, and after the color changes from reddish brown to orange-yellow, transferred to a polytetrafluoroethylene high-pressure reactor, hydrothermally reacted at 150° C. for 12 hours, centrifuged, washed and dried in sequence to obtain MIL-100 (Fe);

[0045] Step 8. Mix and grind MIL-100 (Fe) and commercial sublimed sulfur in a mass ratio of 1:3, and load the mixture into a single-pass quartz sleeve with a small inner diameter. Nest the tube mouth of one end of the double-pass quartz sleeve with a large inner diameter and the tube mouth of the single-pass quartz sleeve with a small inner diameter. Put the nested quartz sleeves into a tubular furnace filled with nitrogen, so that the tube mouth of the other end of the double-pass quartz sleeve with a large inner diameter faces the nitrogen inlet of the tubular furnace. Heat up from room temperature to 150°C at a heating rate of 5°C / min and keep warm for 1h, then continue to heat up to 400°C at a heating rate of 5°C / min and keep warm for 4h. After cooling, porous FeS2@C nanoparticles are obtained.

[0046] from Figure 2 It can be seen that the XRD diffraction peak of MIL-100(Fe) synthesized in Example 1 corresponds to that of MIL-100(Fe) synthesized by the classical hydrothermal method, indicating that MIL-100(Fe) was successfully prepared.

[0047] from Figure 3 It can be seen that in the XRD spectrum of the FeS2@C nanoparticles prepared in Example 1, the diffraction peaks at 2θ values ​​of 28.52°, 33.05°, 37.08°, 40.77°, 47.43°, 56.28°, 59.02°, 61.69°, and 64.29° are respectively corresponding to the FeS2 crystal plane (ICSD No.: 10422) (200),(102),(112), (113), (302) and (213) correspond to each other, revealing the formation of the FeS2 structure; at the same time, there are no other impurity peaks in the spectrum, which indicates that high-purity FeS2 has been successfully prepared.

[0048] from Figure 4 It can be seen that the FeS2@C nanoparticles prepared in Example 1 are porous and have a small particle size, and have an overall honeycomb porous structure, thereby providing more storage active sites for potassium ions and being able to better adapt to the volume expansion that occurs during the potassium insertion process.

[0049] The porous FeS2@C nanoparticles prepared in Example 1 were mixed with a conductive agent Super-P and a binder PVDF (polyvinylidene fluoride) in a mass ratio of 7:2:1, and then NMP was added as a solvent and stirred thoroughly to obtain a slurry. The slurry was applied to the surface of a carbon-coated aluminum foil and dried at 90°C for 12 h under vacuum conditions. A disc with a diameter of 14 mm was punched out using a punching machine and compacted under 10 MPa to obtain a button-type battery positive electrode sheet, recorded as a FeS2@C positive electrode sheet. In the same way, a button-type battery positive electrode sheet was obtained using commercially available FeS2, recorded as a FeS2 positive electrode sheet.

[0050] In a glove box filled with argon, potassium foil was used as the counter electrode, 1 mol / L KFSI EC / DEC (volume ratio = 1:1) was used as the electrolyte, and a glass fiber separator (GF / D) was used as the battery separator. According to the assembly sequence of button cells, the above-mentioned positive electrode sheet, counter electrode, electrolyte and battery separator were assembled into a button half-cell. The constant current charge and discharge test was carried out at room temperature and a voltage of 0.01 to 3.0 V using the BTS test system of Shenzhen Neware Company. The results are as follows: Figure 5 and Figure 6 As shown;

[0051] Figure 5 The button half-cell assembled with FeS2@C cathode has a voltage window of 0.01-3 V and a scan rate of 0.1 mV s -1 From the five initial cyclic voltammetry (CV) curves under the conditions, it can be seen that two reduction peaks appeared in the first cycle during the cathode scan. The peak at 0.9V means initial potassium insertion, accompanied by the production of KxFeS2, and the peak at 0.5V is attributed to the process of the conversion reaction of KxFeS2 to K2S in the electrode material. In addition, three different oxidation peaks appeared in the first cycle scanning curve of the anode, showing the process of potassium removal. 1.5V and 1.8V indicate that K2S is converted to KxFeS2, and the peak at 2.5V is a sign of FeS2 production. The first discharge has the formation of solid electrolyte interface (SEI) and the occurrence of irreversible side reactions, which leads to large differences in the first cycle curves. From the results of the overlap between the second and fifth cycles, FeS2@C has a high charge and discharge reversibility. Due to its porous structure, it can reduce the influence of electrode material pulverization, so it provides higher reaction reversibility and cycle stability for potassium storage.

[0052] Figure 6 The button half-cell assembled with FeS2@C positive electrode sheet and the button half-cell assembled with FeS2 positive electrode sheet were respectively -1 The cycling curve under current density shows that the button half-cell assembled with FeS2@C positive electrode sheet still maintains 112 mAh g after 1000 cycles. -1The discharge capacity of the button half-cell assembled with FeS2 positive electrode is only 83 mAh g -1 In comparison, it is sufficient to illustrate that the porous FeS2@C nanoparticles prepared in Example 1, when applied to potassium ion batteries, can give potassium ion batteries excellent cycle performance. It can be seen that the porous FeS2@C nanoparticles are promising negative electrode materials for potassium ion batteries.

[0053] Example 2

[0054] Step 1: first remove the outer packaging of the retired lithium iron phosphate battery to expose the aluminum shell, and then immerse the retired lithium iron phosphate battery in a 2M sodium chloride solution and discharge it for 2 days;

[0055] Step 2: dismantle and sort the discharged retired lithium iron phosphate batteries to separate the positive electrode sheets;

[0056] Step 3: Place the positive electrode sheet in a muffle furnace at 500° C. for 2 hours to remove the binder and current collector aluminum foil on the positive electrode sheet and separate the lithium iron phosphate positive electrode powder;

[0057] Step 4, immerse 2g of lithium iron phosphate positive electrode powder in 30mL of 1M hydrochloric acid solution, stir for 4h at 60°C and 300r / min to completely dissolve the lithium iron phosphate, centrifuge and filter to obtain an acid leaching solution containing iron, lithium and phosphate ions;

[0058] Step 5, while stirring the acid leaching solution at a speed of 300 r / min, adding sodium hydroxide solution to the acid leaching solution until the pH value is 6, to obtain a suspension containing iron hydroxide precipitate;

[0059] Step 6, centrifuging, washing and drying the suspension in sequence to obtain pure ferric hydroxide powder;

[0060] Step 7, according to the molar ratio of ferric hydroxide, 1,3,5-benzenetricarboxylic acid, concentrated nitric acid and water of 1:0.67:166:0.6, ferric hydroxide powder, 1,3,5-benzenetricarboxylic acid, water and concentrated nitric acid with a mass fraction of 65% are mixed, stirred at a speed of 400r / min, and after the color changes from reddish brown to orange-yellow, transferred to a polytetrafluoroethylene high-pressure reactor, hydrothermally reacted at 160°C for 18h, centrifuged, washed and dried in sequence to obtain MIL-100(Fe);

[0061] Step 8. Mix and grind MIL-100 (Fe) and commercial sublimed sulfur in a mass ratio of 1:2, and load the mixture into a single-pass quartz sleeve with a small inner diameter. Nest the tube mouth of one end of the double-pass quartz sleeve with a large inner diameter and the tube mouth of the single-pass quartz sleeve with a small inner diameter. Put the nested quartz sleeves into a tubular furnace filled with nitrogen, so that the tube mouth of the other end of the double-pass quartz sleeve with a large inner diameter faces the nitrogen inlet of the tubular furnace. Heat up from room temperature to 100°C at a heating rate of 5°C / min and keep warm for 2h, then continue to heat up to 450°C at a heating rate of 5°C / min and keep warm for 5h. After cooling, porous FeS2@C nanoparticles are obtained.

[0062] Example 3

[0063] Step 1: first remove the outer packaging of the retired lithium iron phosphate battery to expose the aluminum shell, and then immerse the retired lithium iron phosphate battery in a 2M sodium chloride solution and discharge it for 2 days;

[0064] Step 2: dismantle and sort the discharged retired lithium iron phosphate batteries to separate the positive electrode sheets;

[0065] Step 3: Place the positive electrode sheet in a muffle furnace at 600° C. for 1 hour to remove the binder and the current collector aluminum foil on the positive electrode sheet and separate the lithium iron phosphate positive electrode powder;

[0066] Step 4, immerse 3g of lithium iron phosphate positive electrode powder in 45mL of 1M sulfuric acid solution, stir at 70°C and 400r / min for 3h to completely dissolve the lithium iron phosphate, centrifuge and filter to obtain an acid leaching solution containing iron, lithium and phosphate ions;

[0067] Step 5, while stirring the acid leaching solution at a speed of 400 r / min, adding potassium hydroxide solution to the acid leaching solution until the pH value is 6, to obtain a suspension containing iron hydroxide precipitate;

[0068] Step 6, centrifuging, washing and drying the suspension in sequence to obtain pure ferric hydroxide powder;

[0069] Step 7, according to the molar ratio of ferric hydroxide, 1,3,5-benzenetricarboxylic acid, concentrated nitric acid and water of 1:0.67:166:0.6, ferric hydroxide powder, 1,3,5-benzenetricarboxylic acid, water and concentrated nitric acid with a mass fraction of 65% are mixed, stirred at a speed of 500r / min, and after the color changes from reddish brown to orange-yellow, transferred to a polytetrafluoroethylene high-pressure reactor, hydrothermally reacted at 170°C for 15h, centrifuged, washed and dried in sequence to obtain MIL-100(Fe);

[0070] Step 8. Mix and grind MIL-100 (Fe) and commercial sublimed sulfur in a mass ratio of 1:2.5, and load the mixture into a single-pass quartz sleeve with a small inner diameter. Nest the tube mouth of one end of the double-pass quartz sleeve with a large inner diameter and the tube mouth of the single-pass quartz sleeve with a small inner diameter. Put the nested quartz sleeves into a tubular furnace filled with nitrogen, so that the tube mouth of the other end of the double-pass quartz sleeve with a large inner diameter faces the nitrogen inlet of the tubular furnace. Heat up from room temperature to 125°C at a heating rate of 5°C / min and keep warm for 1.5h, then continue to heat up to 500°C at a heating rate of 5°C / min and keep warm for 4h. After cooling, porous FeS2@C nanoparticles are obtained.

[0071] Example 4

[0072] Step 1: first remove the outer packaging of the retired lithium iron phosphate battery to expose the aluminum shell, and then immerse the retired lithium iron phosphate battery in a 2M sodium chloride solution and discharge it for 2 days;

[0073] Step 2: dismantle and sort the discharged retired lithium iron phosphate batteries to separate the positive electrode sheets;

[0074] Step 3: Place the positive electrode sheet in a muffle furnace at 450° C. for 2.5 hours to remove the binder and current collector aluminum foil on the positive electrode sheet and separate the lithium iron phosphate positive electrode powder;

[0075] Step 4, immerse 2g of lithium iron phosphate positive electrode powder in 30mL of 1M hydrochloric acid solution, stir for 4h at 60°C and 300r / min to completely dissolve the lithium iron phosphate, centrifuge and filter to obtain an acid leaching solution containing iron, lithium and phosphate ions;

[0076] Step 5, while stirring the acid leaching solution at a speed of 500 r / min, adding potassium hydroxide solution to the acid leaching solution until the pH value is 4, to obtain a suspension containing iron hydroxide precipitate;

[0077] Step 6, centrifuging, washing and drying the suspension in sequence to obtain pure ferric hydroxide powder;

[0078] Step 7, according to the molar ratio of ferric hydroxide, 1,3,5-benzenetricarboxylic acid, concentrated nitric acid and water of 1:0.67:166:0.6, ferric hydroxide powder, 1,3,5-benzenetricarboxylic acid, water and concentrated nitric acid with a mass fraction of 65% are mixed, stirred at a speed of 400r / min, and after the color changes from reddish brown to orange-yellow, transferred to a polytetrafluoroethylene high-pressure reactor, hydrothermally reacted at 180°C for 10h, centrifuged, washed and dried in sequence to obtain MIL-100(Fe);

[0079] Step 8. Mix and grind MIL-100 (Fe) and commercial sublimed sulfur in a mass ratio of 1:3, and load the mixture into a single-pass quartz sleeve with a small inner diameter. Nest the tube mouth of one end of the double-pass quartz sleeve with a large inner diameter and the tube mouth of the single-pass quartz sleeve with a small inner diameter. Put the nested quartz sleeves into a tubular furnace filled with nitrogen, so that the tube mouth of the other end of the double-pass quartz sleeve with a large inner diameter faces the nitrogen inlet of the tubular furnace. Heat up from room temperature to 130°C at a heating rate of 5°C / min and keep warm for 2h, then continue to heat up to 400°C at a heating rate of 5°C / min and keep warm for 5h. After cooling, porous FeS2@C nanoparticles are obtained.

[0080] Example 5

[0081] Step 1: first remove the outer packaging of the retired lithium iron phosphate battery to expose the aluminum shell, and then immerse the retired lithium iron phosphate battery in a 2M sodium chloride solution and discharge it for 2 days;

[0082] Step 2: dismantle and sort the discharged retired lithium iron phosphate batteries to separate the positive electrode sheets;

[0083] Step 3: Place the positive electrode sheet in a muffle furnace at 550° C. for 1.5 hours to remove the binder and current collector aluminum foil on the positive electrode sheet and separate the lithium iron phosphate positive electrode powder;

[0084] Step 4, immerse 1.5g of lithium iron phosphate positive electrode powder in 20mL of 1M sulfuric acid solution, stir at 50°C and 600r / min for 2h to completely dissolve the lithium iron phosphate, centrifuge and filter to obtain an acid leaching solution containing iron, lithium and phosphate ions;

[0085] Step 5, while stirring the acid leaching solution at a speed of 500 r / min, adding sodium hydroxide solution to the acid leaching solution until the pH value is 5, to obtain a suspension containing iron hydroxide precipitate;

[0086] Step 6, centrifuging, washing and drying the suspension in sequence to obtain pure ferric hydroxide powder;

[0087] Step 7, according to the molar ratio of ferric hydroxide, 1,3,5-benzenetricarboxylic acid, concentrated nitric acid and water of 1:0.67:166:0.6, ferric hydroxide powder, 1,3,5-benzenetricarboxylic acid, water and concentrated nitric acid with a mass fraction of 65% are mixed, stirred at a speed of 400r / min, and after the color changes from reddish brown to orange-yellow, transferred to a polytetrafluoroethylene high-pressure reactor, hydrothermally reacted at 160°C for 18h, centrifuged, washed and dried in sequence to obtain MIL-100(Fe);

[0088] Step 8. Mix and grind MIL-100 (Fe) and commercial sublimed sulfur in a mass ratio of 1:2, and load the mixture into a single-pass quartz sleeve with a small inner diameter. Nest the tube mouth of one end of the double-pass quartz sleeve with a large inner diameter and the tube mouth of the single-pass quartz sleeve with a small inner diameter. Put the nested quartz sleeves into a tubular furnace filled with nitrogen, so that the tube mouth of the other end of the double-pass quartz sleeve with a large inner diameter faces the nitrogen inlet of the tubular furnace. Heat up from room temperature to 150°C at a heating rate of 5°C / min and keep warm for 1h, then continue to heat up to 450°C at a heating rate of 5°C / min and keep warm for 5h. After cooling, porous FeS2@C nanoparticles are obtained.

[0089] Example 6

[0090] Step 1: first remove the outer packaging of the retired lithium iron phosphate battery to expose the aluminum shell, and then immerse the retired lithium iron phosphate battery in a 2M sodium chloride solution and discharge it for 2 days;

[0091] Step 2: dismantle and sort the discharged retired lithium iron phosphate batteries to separate the positive electrode sheets;

[0092] Step 3: Place the positive electrode sheet in a muffle furnace at 450° C. for 2.5 hours to remove the binder and current collector aluminum foil on the positive electrode sheet and separate the lithium iron phosphate positive electrode powder;

[0093] Step 4, immerse 2g of lithium iron phosphate positive electrode powder in 30mL of 1M nitric acid solution, stir for 4h at 60°C and 300r / min to completely dissolve the lithium iron phosphate, centrifuge and filter to obtain an acid leaching solution containing iron, lithium and phosphate ions;

[0094] Step 5, while stirring the acid leaching solution at a speed of 500 r / min, adding sodium carbonate solution to the acid leaching solution until the pH value is 4, to obtain a suspension containing iron hydroxide precipitate;

[0095] Step 6, centrifuging, washing and drying the suspension in sequence to obtain pure ferric hydroxide powder;

[0096] Step 7, according to the molar ratio of ferric hydroxide, 1,3,5-benzenetricarboxylic acid, concentrated nitric acid and water of 1:0.67:166:0.6, ferric hydroxide powder, 1,3,5-benzenetricarboxylic acid, water and concentrated nitric acid with a mass fraction of 65% are mixed, stirred at a speed of 400r / min, and after the color changes from reddish brown to orange-yellow, transferred to a polytetrafluoroethylene high-pressure reactor, hydrothermally reacted at 180°C for 10h, centrifuged, washed and dried in sequence to obtain MIL-100(Fe);

[0097] Step 8. Mix and grind MIL-100 (Fe) and commercial sublimed sulfur in a mass ratio of 1:3, and load the mixture into a single-pass quartz sleeve with a small inner diameter. Nest the tube mouth of one end of the double-pass quartz sleeve with a large inner diameter and the tube mouth of the single-pass quartz sleeve with a small inner diameter. Put the nested quartz sleeves into a tubular furnace filled with nitrogen, so that the tube mouth of the other end of the double-pass quartz sleeve with a large inner diameter faces the nitrogen inlet of the tubular furnace. Heat up from room temperature to 130°C at a heating rate of 5°C / min and keep warm for 2h, then continue to heat up to 500°C at a heating rate of 5°C / min and keep warm for 6h. After cooling, porous FeS2@C nanoparticles are obtained.

[0098] Example 7

[0099] Step 1: first remove the outer packaging of the retired lithium iron phosphate battery to expose the aluminum shell, and then immerse the retired lithium iron phosphate battery in a 2M sodium chloride solution and discharge it for 2 days;

[0100] Step 2: dismantle and sort the discharged retired lithium iron phosphate batteries to separate the positive electrode sheets;

[0101] Step 3: Place the positive electrode sheet in a muffle furnace at 450° C. for 2.5 hours to remove the binder and current collector aluminum foil on the positive electrode sheet and separate the lithium iron phosphate positive electrode powder;

[0102] Step 4, immerse 2.5g of lithium iron phosphate positive electrode powder in 35mL of 1M nitric acid solution, stir for 3h at 45°C and 200r / min to completely dissolve the lithium iron phosphate, centrifuge and filter to obtain an acid leaching solution containing iron, lithium and phosphate ions;

[0103] Step 5, while stirring the acid leaching solution at a speed of 200 r / min, adding sodium carbonate solution to the acid leaching solution until the pH value is 5, to obtain a suspension containing iron hydroxide precipitate;

[0104] Step 6, centrifuging, washing and drying the suspension in sequence to obtain pure ferric hydroxide powder;

[0105] Step 7, according to the molar ratio of ferric hydroxide, 1,3,5-benzenetricarboxylic acid, concentrated nitric acid and water of 1:0.67:166:0.6, ferric hydroxide powder, 1,3,5-benzenetricarboxylic acid, water and concentrated nitric acid with a mass fraction of 65% are mixed, stirred at a speed of 300 r / min, and after the color changes from reddish brown to orange-yellow, transferred to a polytetrafluoroethylene high-pressure reactor, hydrothermally reacted at 170° C. for 20 hours, centrifuged, washed and dried in sequence to obtain MIL-100 (Fe);

[0106] Step 8. Mix and grind MIL-100 (Fe) and commercial sublimed sulfur in a mass ratio of 1:2, and load the mixture into a single-pass quartz sleeve with a small inner diameter. Nest the tube mouth of one end of the double-pass quartz sleeve with a large inner diameter and the tube mouth of the single-pass quartz sleeve with a small inner diameter. Put the nested quartz sleeves into a tubular furnace filled with nitrogen, so that the tube mouth of the other end of the double-pass quartz sleeve with a large inner diameter faces the nitrogen inlet of the tubular furnace. Heat up from room temperature to 140°C at a heating rate of 5°C / min and keep warm for 1.5 hours, then continue to heat up to 400°C at a heating rate of 5°C / min and keep warm for 6 hours. After cooling, porous FeS2@C nanoparticles are obtained.

Claims

1. A method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials, characterized in that: The steps include: Step 1: first remove the outer packaging of the retired lithium iron phosphate battery to expose the aluminum shell, and then immerse the retired lithium iron phosphate battery in salt water for discharge; Step 2: dismantle the discharged retired lithium iron phosphate battery and sort out the positive electrode sheet; Step 3: Place the positive electrode sheet in a muffle furnace for calcination to remove the binder and the current collector aluminum foil on the positive electrode sheet and separate the lithium iron phosphate positive electrode powder; Step 4, immerse 1-3 g of lithium iron phosphate positive electrode powder in 15-45 mL of an acidic solution with a concentration of 1 M, stir at 45-70° C. to completely dissolve the lithium iron phosphate, centrifuge and filter to obtain an acid leaching solution containing iron, lithium and phosphate ions; Step 5, while stirring the acid leaching solution, add an alkaline solution to the acid leaching solution until the pH value is 4 to 6, to obtain a suspension containing iron hydroxide precipitate; Step 6, centrifuging, washing and drying the suspension in sequence to obtain pure ferric hydroxide powder; Step 7, according to the molar ratio of ferric hydroxide, 1,3,5-benzenetricarboxylic acid, concentrated nitric acid and water of 1:0.67:166:0.6, ferric hydroxide powder, 1,3,5-benzenetricarboxylic acid, water and concentrated nitric acid with a mass fraction of 65% are mixed and stirred evenly, and after the color changes from reddish brown to orange-yellow, the mixture is transferred to a polytetrafluoroethylene high-pressure reactor, and hydrothermally reacted at 150-180° C. for 10-20 hours, and then centrifuged, washed and dried in sequence to obtain MIL-100(Fe); Step 8. Mix and grind MIL-100 (Fe) and commercial sublimed sulfur in a mass ratio of 1: (2-3), put the mixture into a casing, place the casing into a tubular furnace filled with nitrogen, heat the temperature from room temperature to 100-150°C at a heating rate of 5°C / min and keep it warm for 1-2h, then continue to heat the temperature to 400-500°C at a heating rate of 5°C / min and keep it warm for 4-6h. After cooling, porous FeS2@C nanoparticles are obtained.

2. The method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The brine in step 1 is a sodium chloride solution with a concentration of 2M.

3. The method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The calcination in step 3 is carried out at 400-600° C. for 1-3 hours.

4. The method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The acidic solution in step 4 is: sulfuric acid, hydrochloric acid or nitric acid solution.

5. The method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The stirring in step 4 is carried out at a speed of 200 to 600 r / min for 2 to 4 hours.

6. The method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The alkaline solution in step 5 is sodium hydroxide, potassium hydroxide or sodium carbonate solution.

7. The method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The stirring in step 5 is carried out at a rotation speed of 200 to 600 r / min.

8. The method for preparing porous FeS2@C nanoparticles using retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The sleeve in step 8 is a quartz sleeve, and the tube mouth of the sleeve faces the nitrogen inlet of the tube furnace.

9. Porous FeS2@C nanoparticles prepared by the method according to any one of claims 1 to 8.

10. Use of the porous FeS2@C nanoparticles according to claim 8 as a negative electrode material for potassium ion batteries.

Citation Information

Cited By

  • Method for reversely analyzing particle size of lithium iron phosphate of positive pole piece