Preparation method and application of nickel-cobalt-manganese precursor and positive electrode material

Through the gradient distribution and surface modification treatment of nickel-cobalt-manganese precursor, a single-component polymorphic lithium-rich manganese-based cathode material was prepared, which solved the problem of poor thermal stability of lithium-ion batteries and achieved high energy density and long-life lithium ions. Battery applications.

CN118724085AInactive Publication Date: 2024-10-01NINGBO FULI BATTERY MATERIAL TECH CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411212137.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The high energy density requirements of existing lithium-ion batteries result in poor thermal stability of the cathode material, which can easily cause oxygen release and thermal runaway, limiting its application in large-scale energy storage fields such as electric vehicles.

Method used

Using a nickel-cobalt-manganese precursor preparation method, by configuring nickel-cobalt-manganese mixed salt solutions in different proportions, and performing a co-precipitation reaction, a gradient-distributed nickel-cobalt-manganese precursor with high internal Mn element content and low surface Mn element content is obtained. , mixed and sintered with the lithium source solid phase, and surface modified to prepare a single-component polymorphic lithium-rich manganese-based cathode material.

Benefits of technology

This method maintains high discharge capacity while significantly improving the thermal stability of the cathode material, ensuring high efficiency and long cycle life of the full battery without generating gas during the charging process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724085A_ABST
    Figure CN118724085A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a nickel-cobalt-manganese precursor and a lithium-rich manganese-based positive electrode material. According to the method, a gradient distribution nickel-cobalt-manganese precursor with high internal Mn element content and low surface Mn element content is designed, the nickel-cobalt-manganese precursor and a lithium source are subjected to solid-phase mixing and sintering, and after surface modification treatment, the lithium-rich manganese-based positive electrode material is obtained. The single-composition polymorphic lithium-rich manganese-based positive electrode material has the same Mn element content, so that relatively high discharge capacity of the lithium-rich manganese-based positive electrode material can be maintained, meanwhile, oxygen release is relieved in the charging process, and the thermal stability is greatly improved; and the lithium ion battery with high safety, high specific energy and long service life can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of positive electrode material preparation, and in particular relates to a method for preparing a nickel-cobalt-manganese precursor and a positive electrode material and applications thereof, and more specifically relates to a method for preparing a nickel-cobalt-manganese precursor and a method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and applications thereof. Background Art

[0002] Among various green energy sources, lithium-ion batteries, as a chemical power source with high specific energy density, cyclic charging and discharging, and environmental friendliness, have been widely used in 3C fields such as mobile phones and computers, and have become one of the strong candidates for power sources for hybrid and pure electric vehicles. The energy density that can be achieved by common lithium-ion secondary batteries is <300 Wh / kg, which cannot meet the requirements of the cruising range of pure electric vehicles. Therefore, it is necessary to greatly increase the energy density of existing batteries. However, increasing the energy density of batteries will reduce their safety, easily causing thermal runaway and explosion, which seriously limits the application of lithium-ion batteries in large-scale energy storage fields such as electric vehicles. In terms of energy density, high-energy-density lithium-ion batteries often require high-specific-energy positive and negative electrode materials. Therefore, in recent years, high-discharge specific-capacity positive electrode materials have attracted more and more attention from researchers. In particular, high-specific-capacity lithium-manganese-rich positive electrode materials are more sought after because of their high discharge capacity. The high capacity of lithium-rich manganese-based positive electrode materials comes from the oxygen-active lattice oxygen that contributes to its high capacity. The lattice oxygen comes from the highly active lithium-rich phase (Li2MnO3). Generally, the higher the proportion of lithium-rich phase (Li2MnO3) in the lithium-rich material, the higher the capacity of the lithium-rich material. The problem is that as the proportion of lithium-rich phase (Li2MnO3) increases, that is, the Mn content increases, the thermal decomposition temperature of the material becomes lower, that is, the thermal stability becomes worse. The positive electrode material is prone to oxygen release during the cycle, which increases the risk of thermal runaway of the battery and causes the battery safety to deteriorate.

[0003] Alleviating oxygen release can fundamentally improve the thermal stability of lithium-rich manganese-based cathode materials and improve battery safety. In recent years, many attempts have been made at home and abroad to dope and coat lithium-rich manganese-based cathode materials, but the above modification methods inevitably sacrifice part of the discharge capacity and reduce the battery energy density. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a method for preparing a nickel-cobalt-manganese precursor and a positive electrode material and an application thereof. The method prepares a single-composition polymorphic lithium-rich manganese-based positive electrode material with a gradient distribution of high internal Mn element content and low surface Mn element content. Compared with traditional lithium-rich manganese-based positive electrode materials, the single-composition polymorphic lithium-rich manganese-based positive electrode material has the same Mn element content and can maintain a higher discharge capacity of the lithium-rich manganese-based positive electrode material. At the same time, during the charging process, the low manganese on the surface effectively inhibits the oxidation of lattice oxygen, thereby effectively alleviating oxygen release and greatly improving thermal stability.

[0005] The present invention provides a method for preparing a nickel-cobalt-manganese precursor, comprising the following steps:

[0006] A series of nickel-cobalt-manganese mixed salt solutions with different proportions are prepared, which are recorded as mixed salt solution 1, mixed salt solution 2, mixed salt solution 3 to mixed solution n; the manganese element concentration in mixed salt solution 1 → mixed salt solution n shows a gradient change trend;

[0007] The mixed solution 1 is metered and pumped into the mixed salt solution 2 to obtain a mixed solution A; the mixed solution A is metered and pumped into the mixed salt solution 3 to obtain a mixed solution B; and the steps are repeated successively until the mixed solution is mixed with the mixed solution N to obtain a mixed solution;

[0008] The mixed solution, the precipitant and the complexing agent are mixed by metering pumping and then subjected to coprecipitation reaction to obtain a nickel-cobalt-manganese precursor suspension;

[0009] Washing, filtering and drying the nickel-cobalt-manganese precursor suspension to obtain a nickel-cobalt-manganese precursor;

[0010] The nickel-cobalt-manganese precursor has a composition of Formula 101, Formula 102 or Formula 103:

[0011] Ni a0 Co b0 Mn c0 CO3 formula 101;

[0012] Ni a0 Co b0 Mn c0 (OH)2 formula 102;

[0013] Ni a0 Co b0 Mn c0 (COOH)2 formula 103;

[0014] Among them, 0 <a0≤0.5,0≤b0<0.5,0.5≤c0<1。

[0015] Preferably, the temperature of the coprecipitation reaction is 45-60°C;

[0016] The coprecipitation reaction was carried out under stirring conditions with a stirring rate of 400-800 rpm;

[0017] The pH value of the coprecipitation reaction is 7.5~11;

[0018] The coprecipitation reaction time is 40~140h.

[0019] Preferably, the precipitant is a water-soluble carbonate, a water-soluble acetate or a water-soluble hydroxide.

[0020] Preferably, the nickel-cobalt-manganese precursor is a secondary spherical particle formed by stacking primary lamellar particles;

[0021] The particle size D50 of the primary sheet particles is 50-500 nm;

[0022] The particle size D50 of the secondary spherical particles is 3 μm to 30 μm;

[0023] The specific surface area of ​​the nickel-cobalt-manganese precursor is 1 to 85 m 2 / g.

[0024] The present invention provides a method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material, comprising the following steps:

[0025] The nickel-cobalt-manganese precursor described in the above technical solution is mixed with a lithium source in a solid phase and sintered to obtain Li d Ni x Co y Mn z O2; where d>1, 0.5≤z<1, 0.1 <x<0.5,0<y<1;

[0026] Li d Ni x Co y Mn z O2 surface modification treatment to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material;

[0027] The single-composition multi-morphology lithium-rich manganese-based positive electrode material has a composition of Li d Ni a Co b Mn c O2;0 <a≤0.5,0≤b<0.5,0.5≤c<1。

[0028] Preferably, the lithium-rich manganese-based positive electrode material is composed of the following substances:

[0029] x1 Li d1 Ni a1 Co b1 Mn c1 O2, x2 Lid2 Ni a2 Co b2 Mn c2 O2, x3 Li d3 Ni a3 Co b3 Mn c3 O2、······xn Li dn Ni an Co bn Mn cn O2, formula I, where n≥2;

[0030] x1+ x2+ x3+…+ xn=1;

[0031] a1+a2+a3+…+an=a;

[0032] b1+b2+b3+…+bn=b;

[0033] c1+c2+c3+……+cn=c;

[0034] d1+d2+d3+……+dn=d.

[0035] The present invention provides a positive electrode plate, which is prepared by coating a slurry made of a single-composition multi-morphological lithium-manganese-rich positive electrode material prepared by the preparation method described in the above technical solution, a conductive agent, a binder and a solvent.

[0036] The present invention provides a lithium-ion battery, comprising the positive electrode sheet described in the above technical solution;

[0037] and a negative electrode;

[0038] The active material on the negative electrode plate is selected from one or more of graphite, artificial graphite, silicon-carbon material, lithium metal negative electrode and lithium-carbon negative electrode material.

[0039] The invention provides a method for preparing a nickel-cobalt-manganese precursor, comprising the following steps: preparing a series of nickel-cobalt-manganese mixed salt solutions in different proportions, recorded as mixed salt solution 1, mixed salt solution 2, mixed salt solution 3 until mixed solution n; the manganese element concentration in mixed salt solution 1→mixed salt solution n presents a gradient change trend; metering and pumping the mixed solution 1 into the mixed salt solution 2 to obtain a mixed solution A; metering and pumping the mixed solution A into the mixed salt solution 3 to obtain a mixed solution B; and sequentially performing the steps until the mixed solution is mixed with the mixed solution N to obtain a mixed solution; and metering and pumping the mixed solution, a precipitant and a complexing agent into the mixed solution, and then performing a coprecipitation reaction to obtain a nickel-cobalt-manganese precursor. The nickel-cobalt-manganese precursor prepared by this method is a material with a high internal Mn content and a low surface Mn content. After solid-phase mixing and sintering with a lithium source and surface modification, a single-composition multi-morphology lithium-rich manganese-based positive electrode material is obtained. Compared with traditional lithium-rich manganese-based positive electrode materials, the single-composition multi-morphology lithium-rich manganese-based positive electrode material has the same Mn content, so it can maintain a higher discharge capacity of the lithium-rich manganese-based positive electrode material. At the same time, it can alleviate oxygen release during charging and greatly improve thermal stability. The first cycle efficiency of the full battery assembled with the positive electrode material prepared by this method reaches more than 85%; the energy density of the battery is between 305 and 380 Wh / Kg when the full battery is in the voltage range of 2~4.55V and 0.1C discharge; the full battery is cycled for at least 800 cycles in the voltage range of 2.3~4.5V, and the capacity retention rate is more than 80%; and no gas is produced during the cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 The figure is a schematic diagram of the process of obtaining a mixed solution in the present invention. DETAILED DESCRIPTION

[0041] The present invention provides a method for preparing a nickel-cobalt-manganese precursor, comprising the following steps:

[0042] A series of nickel-cobalt-manganese mixed salt solutions with different proportions are prepared, which are recorded as mixed salt solution 1, mixed salt solution 2, mixed salt solution 3 to mixed solution n; the manganese element concentration in mixed salt solution 1 → mixed salt solution n shows a gradient change trend;

[0043] The mixed solution 1 is metered and pumped into the mixed salt solution 2 to obtain a mixed solution A; the mixed solution A is metered and pumped into the mixed salt solution 3 to obtain a mixed solution B; and the steps are repeated successively until the mixed solution is mixed with the mixed solution N to obtain a mixed solution;

[0044] The mixed solution, the precipitant and the complexing agent are mixed by metering pumping and then subjected to coprecipitation reaction to obtain a nickel-cobalt-manganese precursor suspension;

[0045] Washing, filtering and drying the nickel-cobalt-manganese precursor suspension to obtain a nickel-cobalt-manganese precursor;

[0046] The nickel-cobalt-manganese precursor has a composition of Formula 101, Formula 102 or Formula 103:

[0047] Ni a0 Co b0 Mn c0 CO3 formula 101;

[0048] Ni a0 Co b0 Mn c0 (OH)2 formula 102;

[0049] Ni a0 Co b0 Mn c0 (COOH)2 formula 103;

[0050] Among them, 0 <a0≤0.5,0≤b0<0.5,0.5≤c0<1。

[0051] The nickel-cobalt-manganese precursor prepared by the method provided by the present invention is a material with a high internal Mn content and a low surface Mn content. After solid phase mixing and sintering with a lithium source, and then surface modification treatment, a single-composition multi-morphology lithium-rich manganese-based positive electrode material is obtained. Compared with the traditional lithium-rich manganese-based positive electrode material, the single-composition multi-morphology lithium-rich manganese-based positive electrode material has the same Mn element content, so it can maintain a higher discharge capacity of the lithium-rich manganese-based positive electrode material. At the same time, it alleviates oxygen release during charging and greatly improves thermal stability. The first cycle efficiency of the full battery assembled with the positive electrode material prepared by the method reaches more than 85%; the energy density of the battery is between 305 and 380 Wh / Kg when the full battery is in the voltage range of 2~4.55V and 0.1C discharge; the full battery is cycled for at least 800 cycles in the voltage range of 2.3~4.5V, and the capacity retention rate is more than 80%; and no gas is produced during the cycle.

[0052] The present invention first configures a series of nickel-cobalt-manganese mixed salt solutions of different proportions, recorded as mixed salt solution 1, mixed salt solution 2, mixed salt solution 3 until mixed solution n; the manganese concentration in mixed salt solution 1→mixed salt solution n shows a gradient change trend. The trend of the gradient change is to increase or decrease. The molar ratio of nickel to cobalt in the mixed salt solution is preferably 1:1. For example, in a specific embodiment, 1:1:1, 1:1:4, 1:1:7; or 1:1:1, 1:1:2, 1:1:6; or 1:1:1, 1:1:3, 1:1:5, 1:1:7, 1:1:9; or 1:1:1, 1:1:2, 1:1:7; or 1:1:1, 1:1:7; or nickel:manganese=2:5, 2:7; or nickel:manganese=1:1, 1:3.

[0053] See also Figure 1 , Figure 1 The schematic diagram of the process of obtaining a mixed solution of the present invention is as follows: Mixed solution 1 is metered and pumped into mixed salt solution 2 to obtain mixed solution A; mixed solution A is metered and pumped into mixed salt solution 3 to obtain mixed solution B; and the process is repeated until mixed with mixed solution N to obtain a mixed solution.

[0054] After obtaining the mixed solution, the present invention mixes the mixed solution, the precipitant and the complexing agent by metering pumping, and then performs a coprecipitation reaction to obtain a nickel-cobalt-manganese precursor suspension. The precipitant in the present invention is sodium carbonate, sodium hydroxide or sodium acetate. In a specific embodiment, the pumping flow rate is 0.5 mL / min-4 mL / min. The temperature of the coprecipitation reaction is 45-60°C; the coprecipitation reaction is carried out under stirring conditions, and the stirring rate is 400-800 rpm; the pH value of the coprecipitation reaction is 7.5-11; and the time of the coprecipitation reaction is 40-140 hours. In a specific embodiment, the temperature of the coprecipitation reaction is 56°C, 55°C, 57°C or 48°C; the stirring rate is 750 rpm, 650 rpm or 450 rpm; the pH value is 8.5, 8.2, 8.0, 8.9 or 10.9; and the time of the coprecipitation is 45 hours, 120 hours or 140 hours.

[0055] The present invention washes, filters and dries the nickel-cobalt-manganese precursor suspension to obtain a nickel-cobalt-manganese precursor. The nickel-cobalt-manganese precursor is a secondary spherical particle formed by stacking primary lamellar particles. The particle size D50 of the primary lamellar particles is 50-500nm; the particle size D50 of the secondary spherical particles is 3μm-30μm; the specific surface area of ​​the nickel-cobalt-manganese precursor is 1-85m 2 / g. In a specific embodiment, the particle size D50 of the primary lamellar particles is 200nm, 300nm, 260nm, 60nm, or 100nm; the particle size D50 of the secondary spherical particles is 5.5μm, 10μm, 6μm, 12μm, 22μm, 6.5μm, or 20μm; the specific surface area of ​​the nickel-cobalt-manganese precursor is 65m 2 / g, 55m 2 / g, 81 m 2 / g, 45 m 2 / g, 85 m 2 / g, 75m 2 / g, or 67 m 2 / g.

[0056] In the present invention, if the precipitant is sodium carbonate, the composition of the nickel-cobalt-manganese precursor is Mn c0 Ni a0 Co b0 CO3; if the precipitant is sodium hydroxide, the composition of the nickel-cobalt-manganese precursor is Mn c0 Ni a0 Cob0 (OH)2; if the precipitant is sodium acetate, the composition of the nickel-cobalt-manganese precursor is Mn c0 Ni a0 Co b0 (COOH)2.

[0057] That is to say, the nickel-cobalt-manganese precursor obtained in the present invention has a composition of Formula 101, Formula 102 or Formula 103:

[0058] Ni a0 Co b0 Mn c0 CO3 formula 101;

[0059] Ni a0 Co b0 Mn c0 (OH)2 formula 102;

[0060] Ni a0 Co b0 Mn c0 (COOH)2 formula 103;

[0061] Among them, 0 <a0≤0.5,0≤b0<0.5,0.5≤c0<1。

[0062] The present invention provides a method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material, comprising the following steps:

[0063] The nickel-cobalt-manganese precursor described in the above technical solution is mixed with a lithium source in a solid phase and sintered to obtain Li d Ni x Co y Mn z O2; where 1<d<1.5, 0.5≤z<1, 0.1 <x<0.5,0<y<1;

[0064] Li d Ni x Co y Mn z O2 surface modification treatment to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material;

[0065] The single-composition multi-morphology lithium-rich manganese-based positive electrode material has a composition of Li d Ni a Co b Mn c O2;0 <a≤0.5,0≤b<0.5,0.5≤c<1。

[0066] The present invention mixes the nickel-cobalt-manganese precursor described in the above technical solution with a lithium source and sinters them in a solid phase to obtain Li d Ni xCo y Mn z O2; where d>1,0.1 <x<0.5,0<y<1,0.5≤z<1,x+y+z+d≤2。

[0067] Li d Ni x Co y Mn z O2 surface modification treatment is performed to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material. The surface modification treatment mainly includes steps such as delithiation, coating, and washing.

[0068] In the present invention, the lithium-rich manganese-based positive electrode material is composed of the following substances:

[0069] x1 Li d1 Ni a1 Co b1 Mn c1 O2, x2 Li d2 Ni a2 Co b2 Mn c2 O2, x3 Li d3 Ni a3 Co b3 Mn c3 O2、······xn Li dn Ni an Co bn Mn cn O2, where n ≥ 2;

[0070] x1+ x2+ x3+…+ xn=1;

[0071] a1+a2+a3+…+an=a;

[0072] b1+b2+b3+…+bn=b;

[0073] c1+c2+c3+……+cn=c;

[0074] d1+d2+d3+……+dn=d.

[0075] The thermal stability of the multi-morphologically distributed lithium-rich manganese-based positive electrode material prepared by the present invention is superior to that of the single-morphological lithium-rich manganese-based positive electrode material with the same composition.

[0076] The present invention provides a positive electrode plate, which is prepared by coating a slurry made of a single-composition multi-morphological lithium-manganese-rich positive electrode material prepared by the preparation method described in the above technical solution, a conductive agent, a binder and a solvent.

[0077] The present invention provides a lithium-ion battery, comprising the positive electrode sheet described in the above technical solution;

[0078] and a negative electrode;

[0079] The active material on the negative electrode plate is selected from one or more of graphite, artificial graphite, silicon-carbon material, lithium metal negative electrode, and lithium-carbon negative electrode material.

[0080] The active material of the negative electrode in the present invention is preferably a silicon-carbon material, a lithium metal negative electrode, or a lithium-carbon negative electrode material to form a high-energy-density power battery.

[0081] The present invention adopts the single-composition multi-morphological lithium-rich manganese-based positive electrode material prepared by the above method as the positive electrode material of the lithium-ion battery. The lithium-rich manganese-based positive electrode material with high capacity, high safety, long cycle and high compaction is suitable for preparing high energy density and long life lithium-ion batteries.

[0082] The negative electrode in the present invention also includes a conductive agent, a binder and a solvent; the conductive agent is a mixture of SP and carbon nanotubes; the binder is CMC or PVDF, and the solvent is SBR or NMP.

[0083] The positive and negative electrode sheets are assembled into a battery cell by lamination or winding; the battery cell is baked, injected with electrolyte, and formed to obtain a lithium-ion battery.

[0084] In order to further illustrate the present invention, the preparation method and application of a nickel-cobalt-manganese precursor and a positive electrode material provided by the present invention are described in detail below in combination with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0085] Example 1

[0086] Precursor preparation:

[0087] A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and its application, comprising the following steps:

[0088] (1) preparing 2 mol / L mixed salt solution 1 of 50 L, mixed salt solution 2 of 50 L, and mixed salt solution 3 of 50 L by mixing nickel sulfate, cobalt sulfate, and manganese sulfate in a ratio of 1:1:1, 1:1:4, and 1:1:7, respectively;

[0089] (2) adding the mixed salt solution 1 to the mixed salt solution 2 through a metering pump at a flow rate of 2 mL / min to obtain a mixed solution A, and adding the mixed salt solution 3 to the mixed solution A through a metering pump at a flow rate of 3 mL / min to obtain a mixed solution B;

[0090] (3) preparing a 2 mol / L sodium carbonate solution as a precipitant and a 0.8 mol / L ammonia solution as a complexing agent;

[0091] (4) adding the mixed solution B at 3 mL / min, the complexing agent at 1 mL / min, and the precipitant at a certain speed into a coprecipitation reactor through a metering pump, controlling the reactor temperature at 56° C., the stirring speed at 750 r / min, and the reaction pH at about 8.5, and performing the coprecipitation reaction for 45 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0092] (5) Wash, filter and dry the above-mentioned material precursor suspension to obtain Ni 0.167 Co 0.167 Mn 0.666 CO3 is used to form a nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor; the precursor is a secondary spherical particle formed by stacking primary lamellar particles; the particle size D50 of the primary lamellar particles is 200nm; the particle size D50 of the secondary spherical particles is 5.5μm; the specific surface area of ​​the nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor is 65m 2 / g;

[0093] Cathode material preparation:

[0094] (6) The above-mentioned single-component nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor contains Ni 0.167 Co 0.167 Mn 0.167 CO3 and lithium carbonate are mixed in a solid phase at a molar ratio of Li:Me (the sum of the three elements of nickel, cobalt and manganese) = 1.45, and sintered at a high temperature of 870°C for 16 hours to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material matrix oxide material;

[0095] (7) subjecting the above-mentioned single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material to surface modification treatment to obtain a single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material;

[0096] Positive electrode preparation:

[0097] (8) 95% by weight of the above-mentioned single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material is added together with 3.5% of conductive agent SP+carbon nanotubes (mass ratio 6:1), 1.5% of binder PVDF, and solvent NMP, and added into a batching kettle and stirred to obtain a lithium-ion battery composite positive electrode material slurry;

[0098] (9) coating the single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material slurry on the positive electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the positive electrode material electrode sheet for standby use;

[0099] Negative electrode sheet preparation:

[0100] (10) Similarly, the negative electrode active material silicon-carbon composite negative electrode material (whose discharge capacity is 820 mAh / g), the conductive agent SP+carbon nanotubes (mass ratio 2:1), the binder CMC, and the solvent SBR are mixed at a ratio of 93.5:1.5:1:4, and 70% of the total amount of solvent water is added into a batching kettle for stirring to obtain a lithium ion battery negative electrode material slurry;

[0101] (11) coating the negative electrode material slurry on the negative electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the negative electrode material electrode sheet for standby use;

[0102] Battery preparation:

[0103] (12) Assemble the above positive and negative electrode sheets into a 25Ah battery cell by lamination or winding;

[0104] (13) baking the battery cell, injecting electrolyte, and forming the battery cell to obtain a lithium-ion battery;

[0105] Performance Testing:

[0106] (14) The battery is charged to above 4.55 V for the first cycle and then activated and cycled within a voltage range of 2.3 to 4.5 V.

[0107] Test results:

[0108] After testing, the tap density of the above material reached 2.0 g / cc and the specific surface area of ​​the material was 6.85m 2 / g, the material's first cycle discharge capacity reaches 301mAh / g in the half-cell voltage range of 2~4.8V, and the material's first coulombic efficiency reaches 92% in the half-cell. The compaction density of the positive electrode sheet prepared in the above step (8) is as high as 2.95 g / cc, and the first efficiency of the assembled full battery reaches 90%. In the full battery voltage range of 2~4.55V, the battery's energy density reaches 375Wh / Kg when discharged at 0.1C, and the full battery voltage range of 2.3~4.5V cycles 800 cycles The capacity retention rate is 90%, and no gas is generated during the cycle, which is suitable for the basic needs of high specific energy power battery applications.

[0109] Example 2

[0110] Precursor preparation:

[0111] A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and its application, comprising the following steps:

[0112] (1) preparing 2 mol / L mixed salt solution 1 of 50 L, mixed salt solution 2 of 50 L, and mixed salt solution 3 of 50 L by mixing nickel sulfate, cobalt sulfate, and manganese sulfate in a ratio of 1:1:1, 1:1:2, and 1:1:6, respectively;

[0113] (2) adding the mixed salt solution 1 to the mixed salt solution 2 through a metering pump at a flow rate of 2 mL / min to obtain a mixed solution A, and adding the mixed salt solution 3 to the mixed solution A through a metering pump at a flow rate of 3 mL / min to obtain a mixed solution B;

[0114] (3) preparing a 2 mol / L sodium carbonate solution as a precipitant and a 0.5 mol / L ammonia solution as a complexing agent;

[0115] (4) adding the mixed solution B at 3 mL / min, the complexing agent at 0.5 mL / min, and the precipitant at a certain speed into a coprecipitation reactor through a metering pump, controlling the reactor temperature at 55° C., the stirring speed at 750 r / min, and the reaction pH at about 8.2, and performing the coprecipitation reaction for 45 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0116] (5) Wash, filter and dry the above-mentioned material precursor suspension to obtain Ni 0.2 Co 0.2 Mn 0.6 CO3 is used to form a nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor; the precursor is a secondary spherical particle formed by stacking primary lamellar particles; the particle size D50 of the primary lamellar particles is 100nm; the particle size D50 of the secondary spherical particles is 10μm; the specific surface area of ​​the nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor is 55m 2 / g;

[0117] Cathode material preparation:

[0118] (6) The above-mentioned single-component nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor contains Ni 0.2 Co 0.2 Mn 0.6 CO3 and lithium carbonate are mixed in a solid phase according to a molar ratio of Li:Me=1.25 and sintered at a high temperature of 830°C for 16 hours to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material matrix oxide material;

[0119] (7) subjecting the above-mentioned single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material to surface modification treatment to obtain a single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material;

[0120] Positive electrode preparation:

[0121] (8) 95% by weight of the above-mentioned single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material is added together with 3.5% of conductive agent SP+carbon nanotubes (mass ratio of 6:1), 1.5% of binder PVDF, and solvent NMP, and added into a batching kettle and stirred to obtain a lithium-ion battery composite positive electrode material slurry;

[0122] (9) coating the single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material slurry on the positive electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the positive electrode material electrode sheet for standby use;

[0123] Negative electrode sheet preparation:

[0124] (10) Similarly, the negative electrode active material silicon-carbon composite negative electrode material (whose discharge capacity is 820 mAh / g), the conductive agent SP+carbon nanotubes (mass ratio is 2:1), the binder CMC, and the solvent SBR are mixed at a ratio of 93.5:1.5:1:4, and 70% of the total amount of solvent water is added into a batching kettle and stirred to obtain a lithium ion battery negative electrode material slurry;

[0125] (11) coating the negative electrode material slurry on the negative electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the negative electrode material electrode sheet for standby use;

[0126] Battery preparation:

[0127] (12) Assemble the above positive and negative electrode sheets into a 25Ah battery cell by lamination or winding;

[0128] (13) baking the battery cell, injecting electrolyte, and forming the battery cell to obtain a lithium-ion battery;

[0129] Performance Testing:

[0130] (14) The battery is charged to above 4.55 V for the first cycle and then activated and cycled within a voltage range of 2.3 to 4.5 V.

[0131] Test results:

[0132] After testing, the tap density of the above material reached 2.2 g / cc and the specific surface area of ​​the material was 3.85m 2 / g, the material's first cycle discharge capacity reaches 282mAh / g in the half-cell voltage range of 2~4.8V, and the material's first coulombic efficiency of the half-cell reaches 92%. The compaction density of the positive electrode sheet prepared in step 8 is as high as 3.2 g / cc, and the first efficiency of the assembled full battery reaches 90%. In the full battery voltage range of 2~4.55V, the battery's energy density reaches 355Wh / Kg at 0.1C discharge, and the full battery voltage range of 2.3~4.5V cycles 1200 cycles The capacity retention rate is 90%, and no gas is produced during the cycle, which is suitable for the basic needs of high-energy-density power battery applications.

[0133] Example 3

[0134] Precursor preparation:

[0135] A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and its application, comprising the following steps:

[0136] (1) preparing 2 mol / L 50 L mixed salt solution 1, 50 L mixed salt solution 2, 50 L mixed salt solution 3, 50 L mixed salt solution 4 and 50 L mixed salt solution 5 by mixing nickel sulfate, cobalt sulfate and manganese sulfate compounds in a ratio of 1:1:1, 1:1:3, 1:1:5, 1:1:7 and 1:1:9 respectively;

[0137] (2) adding the mixed salt solution 1 to the mixed salt solution 2 through a metering pump at a flow rate of 1 mL / min to obtain a mixed solution A, adding the mixed solution A to the mixed salt solution 3 through a metering pump at a flow rate of 2 mL / min to obtain a mixed solution B, adding the mixed solution B to the mixed salt solution 4 through a metering pump at a flow rate of 3 mL / min to obtain a mixed solution C, and adding the mixed solution C to the mixed salt solution 5 through a metering pump at a flow rate of 4 mL / min to obtain a mixed solution D;

[0138] (3) preparing a 2 mol / L sodium carbonate solution as a precipitant and a 0.5 mol / L ammonia solution as a complexing agent;

[0139] (4) adding the mixed solution B at 4 mL / min, the complexing agent at 1.5 mL / min, and the precipitant at a certain speed into a coprecipitation reactor through a metering pump, controlling the reactor temperature at 55° C., the stirring speed at 650 r / min, and the reaction pH at about 8.0, and performing the coprecipitation reaction for 120 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0140] (5) Wash, filter and dry the above-mentioned material precursor suspension to obtain Ni 0.143 Co 0.143 Mn 0.714 CO3 is used to form a nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor; the precursor is a secondary spherical particle formed by stacking primary lamellar particles; the particle size D50 of the primary lamellar particles is 100nm; the particle size D50 of the secondary spherical particles is 6μm; the specific surface area of ​​the nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor is 81m 2 / g;

[0141] Cathode material preparation:

[0142] (6) The above-mentioned single-component nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor contains Ni 0.143 Co 0.143 Mn 0.714CO3 and lithium carbonate are mixed in a solid phase according to a molar ratio of Li:Me=1.55 and sintered at a high temperature of 900°C for 8 hours to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material matrix oxide material;

[0143] (7) subjecting the above-mentioned single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material to surface modification treatment to obtain a single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material;

[0144] Positive electrode preparation:

[0145] (8) 95% by weight of the above-mentioned single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material is added with 3.5% of a conductive agent SP+carbon nanotubes (mass ratio of 6:1), a binder PVDF, and a solvent NMP, and the mixture is added into a batching kettle and stirred to obtain a lithium-ion battery composite positive electrode material slurry;

[0146] (9) coating the single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material slurry on the positive electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the positive electrode material electrode sheet for standby use;

[0147] Negative electrode sheet preparation:

[0148] (10) Similarly, the negative electrode active material silicon-carbon composite negative electrode material (whose discharge capacity is 820 mAh / g), the conductive agent SP+carbon nanotubes (mass ratio is 2:1), the binder CMC, and the solvent SBR are mixed at a ratio of 93.5:1.5:1:4, and 70% of the total amount of solvent water is added into a batching kettle and stirred to obtain a lithium ion battery negative electrode material slurry;

[0149] (11) coating the negative electrode material slurry on the negative electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the negative electrode material electrode sheet for standby use;

[0150] Battery preparation:

[0151] (12) Assemble the above positive and negative electrode sheets into a 25Ah battery cell by lamination or winding;

[0152] (13) baking the battery cell, injecting electrolyte, and forming the battery cell to obtain a lithium-ion battery;

[0153] Performance Testing:

[0154] (14) The battery is charged to above 4.55 V for the first cycle and then activated and cycled within a voltage range of 2.3 to 4.5 V.

[0155] Test results:

[0156] After testing, the tap density of the above material reached 2.2 g / cc and the specific surface area of ​​the material was 7.89m2 / g, the material's first discharge capacity in the half-cell voltage range of 2-4.8V reaches 252mAh / g, and the material's first coulombic efficiency in the half-cell reaches 85%. The compaction density of the positive electrode sheet prepared in step 8 is as high as 2.9 g / cc, and the first efficiency of the assembled full battery reaches 90%. In the full battery voltage range of 2~4.55V, the battery's energy density reaches 315Wh / Kg at 0.1C discharge, and the full battery voltage range of 2.3~4.5V cycles 1200 cycles The capacity retention rate is 82%, and no gas is produced during the cycle, which is suitable for the basic needs of high-energy-density power battery applications.

[0157] Example 4

[0158] Precursor preparation:

[0159] A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and its application, comprising the following steps:

[0160] (1) preparing 50 L of 2 mol / L mixed salt solution 1, 100 L of mixed salt solution 2, and 50 L of mixed salt solution 3 by mixing nickel sulfate, cobalt sulfate, and manganese sulfate compounds in a ratio of 1:1:1, 1:1:2, and 1:1:7, respectively;

[0161] (2) adding the mixed salt solution 1 to the mixed salt solution 2 through a metering pump at a flow rate of 2 mL / min to obtain a mixed solution A, and adding the mixed salt solution 3 to the mixed solution A through a metering pump at a flow rate of 4 mL / min to obtain a mixed solution B;

[0162] (3) preparing a 2 mol / L sodium carbonate solution as a precipitant and a 0.5 mol / L ammonia solution as a complexing agent;

[0163] (4) adding the mixed solution B at 4 mL / min, the complexing agent at 1 mL / min, and the precipitant at a certain speed into a coprecipitation reactor through a metering pump, controlling the reactor temperature at 55° C., the stirring speed at 750 r / min, and the reaction pH at about 8.2, and performing the coprecipitation reaction for 45 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0164] (5) Wash, filter and dry the above-mentioned material precursor suspension to obtain Ni 0.2 Co 0.2 Mn 06 CO3 is used to form a nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor; the precursor is a secondary spherical particle formed by stacking primary lamellar particles; the particle size D50 of the primary lamellar particles is 300nm; the particle size D50 of the secondary spherical particles is 12μm; the specific surface area of ​​the nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor is 45m 2 / g;

[0165] Cathode material preparation:

[0166] (6) The above-mentioned single-component nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor contains Ni 0.2 Co 0.2 Mn 06 CO3 and lithium carbonate are mixed in a solid phase according to a molar ratio of Li:Me=1.25 and sintered at a high temperature of 875°C for 12 hours to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material matrix oxide material;

[0167] (7) subjecting the above-mentioned single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material to surface modification treatment to obtain a single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material;

[0168] Positive electrode preparation:

[0169] (8) 95% by weight of the above-mentioned single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material is added together with 3.5% of conductive agent SP+carbon nanotubes (mass ratio of 6:1), 1.5% of binder PVDF, and solvent NMP, and added into a batching kettle and stirred to obtain a lithium-ion battery composite positive electrode material slurry;

[0170] (9) coating the single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material slurry on the positive electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the positive electrode material electrode sheet for standby use;

[0171] Negative electrode sheet preparation:

[0172] (10) Similarly, the negative electrode active material silicon-carbon composite negative electrode material (whose discharge capacity is 820 mAh / g), the conductive agent SP+carbon nanotubes (mass ratio is 2:1), the binder CMC, and the solvent SBR are mixed at a ratio of 93.5:1.5:1:4, and 70% of the total amount of solvent water is added into a batching kettle and stirred to obtain a lithium ion battery negative electrode material slurry;

[0173] (11) coating the negative electrode material slurry on the negative electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the negative electrode material electrode sheet for standby use;

[0174] Battery preparation:

[0175] (12) Assemble the above positive and negative electrode sheets into a 25Ah battery cell by lamination or winding;

[0176] (13) baking the battery cell, injecting electrolyte, and forming the battery cell to obtain a lithium-ion battery;

[0177] Performance Testing:

[0178] (14) The battery is charged to above 4.55V for the first cycle and then activated and cycled within a voltage range of 2.3-4.5V.

[0179] Test results:

[0180] After testing, the tap density of the above material reached 2.15 g / cc and the specific surface area of ​​the material was 4.55m 2 / g, the material's first discharge capacity in the half-cell voltage range of 2-4.8V reaches 275mAh / g, and the material's first coulombic efficiency in the half-cell reaches 92%. The compaction density of the positive electrode sheet prepared in step 8 is as high as 3.0 g / cc, and the first efficiency of the assembled full battery reaches 90%. In the full-cell voltage range of 2-4.55V, the battery's energy density reaches 353Wh / Kg at 0.1C discharge, and the full-cell voltage range of 2.3-4.5V cycles 1200 cycles The capacity retention rate is 91%, and no gas is produced during the cycle, which is suitable for the basic needs of high-energy-density power battery applications.

[0181] Example 5

[0182] Precursor preparation:

[0183] A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and its application, comprising the following steps:

[0184] (1) preparing 50 L of 2 mol / L mixed salt solution 1 and 50 L of mixed salt solution 2 by mixing nickel sulfate, cobalt sulfate and manganese sulfate in a ratio of 1:1:1 and 1:1:7 respectively;

[0185] (2) adding the mixed salt solution 1 to the mixed salt solution 2 at a flow rate of 2 mL / min through a metering pump to obtain a mixed solution A;

[0186] (3) preparing a 2 mol / L sodium carbonate solution as a precipitant and a 0.8 mol / L ammonia solution as a complexing agent;

[0187] (4) adding the mixed solution B at 2 mL / min, the complexing agent at 0.8 mL / min, and the precipitant at a certain speed into a coprecipitation reactor through a metering pump, controlling the reactor temperature at 56° C., the stirring speed at 750 r / min, and the reaction pH at about 8.5, and performing the coprecipitation reaction for 45 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0188] (5) Wash, filter and dry the above-mentioned material precursor suspension to obtain Ni 0167 Co 0.167 Mn 0.666CO3 is composed of a nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor; the precursor is a secondary spherical particle formed by stacking primary lamellar particles; the particle size D50 of the primary lamellar particles is 260nm; the particle size D50 of the secondary spherical particles is 22μm; the specific surface area of ​​the nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor is 85m 2 / g;

[0189] Cathode material preparation:

[0190] (6) The above-mentioned single-component nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor contains Ni 0.167 Co 0.167 Mn 0.167 CO3 and lithium carbonate are mixed in a solid phase according to a molar ratio of Li:Me=1.45 and sintered at a high temperature of 800°C for 16 hours to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material matrix oxide material;

[0191] (7) subjecting the above-mentioned single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material to surface modification treatment to obtain a single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material;

[0192] Positive electrode preparation:

[0193] (8) 95% by weight of the above-mentioned single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material is added together with 3.5% of conductive agent SP+carbon nanotubes (mass ratio of 6:1), 1.5% of binder PVDF, and solvent NMP, and added into a batching kettle and stirred to obtain a lithium-ion battery composite positive electrode material slurry;

[0194] (9) coating the single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material slurry on the positive electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the positive electrode material electrode sheet for standby use;

[0195] Negative electrode sheet preparation:

[0196] (10) Similarly, the negative electrode active material silicon-carbon composite negative electrode material (whose discharge capacity is 820 mAh / g), the conductive agent SP+carbon nanotubes (mass ratio is 2:1), the binder CMC, and the solvent SBR are mixed at a ratio of 93.5:1.5:1:4, and 70% of the total amount of solvent water is added into a batching kettle and stirred to obtain a lithium ion battery negative electrode material slurry;

[0197] (11) coating the negative electrode material slurry on the negative electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the negative electrode material electrode sheet for standby use;

[0198] Battery preparation:

[0199] (12) Assemble the above positive and negative electrode sheets into a 25Ah battery cell by lamination or winding;

[0200] (13) baking the battery cell, injecting electrolyte, and forming the battery cell to obtain a lithium-ion battery;

[0201] Performance Testing:

[0202] (14) The battery is charged to above 4.55V for the first cycle and then activated and cycled within a voltage range of 2.3-4.5V.

[0203] Test results:

[0204] After testing, the tap density of the above material reached 2. g / cc, and the specific surface area of ​​the material was 7.85m 2 / g, the material's first cycle discharge capacity reaches 302mAh / g in the half-cell voltage range of 2-4.8V, and the material's first coulombic efficiency of the half-cell reaches 92%. The compaction density of the positive electrode sheet prepared in the above step (8) is as high as 2.97 g / cc, and the first efficiency of the assembled full battery reaches 90%. In the full battery voltage range of 2~4.55V, the battery's energy density reaches 380Wh / Kg when discharged at 0.1C, and the full battery voltage range of 2.3~4.5V cycles 800 cycles The capacity retention rate is 92%, and no gas is generated during the cycle, which is suitable for the basic application needs of high-energy-density power batteries.

[0205] Example 6

[0206] Precursor preparation:

[0207] A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and its application, comprising the following steps:

[0208] (1) preparing 50 L of 2 mol / L mixed salt solution 1 and 50 L of 2 mol / L mixed salt solution 2 by mixing nickel sulfate and manganese sulfate in a ratio of 2:5 and 2:7 respectively;

[0209] (2) adding the mixed salt solution 1 to the mixed salt solution 2 at a flow rate of 2 mL / min through a metering pump to obtain a mixed solution A;

[0210] (3) preparing a 2 mol / L sodium carbonate solution as a precipitant and a 0.8 mol / L ammonia solution as a complexing agent;

[0211] (4) adding the mixed solution B at 2 mL / min, the complexing agent at 1 mL / min, and the precipitant at a certain speed into a coprecipitation reactor through a metering pump, controlling the reactor temperature at 57° C., the stirring speed at 750 r / min, and the reaction pH at about 8.9, and performing the coprecipitation reaction for 45 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0212] (5) Wash, filter and dry the above-mentioned material precursor suspension to obtain Ni 0.25 Mn 0.75 CO3 is used to form a nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor; the precursor is a secondary spherical particle formed by stacking primary lamellar particles; the particle size D50 of the primary lamellar particles is 60nm; the particle size D50 of the secondary spherical particles is 6.5μm; the specific surface area of ​​the nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor is 75m 2 / g;

[0213] Cathode material preparation:

[0214] (6) The above-mentioned single-component nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor contains Ni 0.25 Mn 0.75 CO3 and lithium carbonate are mixed in a solid phase according to a molar ratio of Li:Me=1.5 and sintered at 900°C for 10 hours to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material matrix oxide material;

[0215] (7) subjecting the above-mentioned single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material to surface modification treatment to obtain a single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material;

[0216] Positive electrode preparation:

[0217] (8) 95% by weight of the above-mentioned single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material is added together with 3.5% of conductive agent SP+carbon nanotubes (mass ratio of 6:1), 1.5% of binder PVDF, and solvent NMP, and added into a batching kettle and stirred to obtain a lithium-ion battery composite positive electrode material slurry;

[0218] (9) coating the single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material slurry on the positive electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the positive electrode material electrode sheet for standby use;

[0219] Negative electrode sheet preparation:

[0220] (10) Similarly, the negative electrode active material silicon-carbon composite negative electrode material (whose discharge capacity is 820 mAh / g), the conductive agent SP+carbon nanotubes (mass ratio is 2:1), the binder CMC, and the solvent SBR are mixed at a ratio of 93.5:1.5:1:4, and 70% of the total amount of solvent water is added into a batching kettle and stirred to obtain a lithium ion battery negative electrode material slurry;

[0221] (11) coating the negative electrode material slurry on the negative electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the negative electrode material electrode sheet for standby use;

[0222] Battery preparation:

[0223] (12) Assemble the above positive and negative electrode sheets into a 25Ah battery cell by lamination or winding;

[0224] (13) baking the battery cell, injecting electrolyte, and forming the battery cell to obtain a lithium-ion battery;

[0225] Performance Testing:

[0226] (14) The battery is charged to above 4.55 V for the first cycle and then activated and cycled within a voltage range of 2.3 to 4.5 V.

[0227] Test results:

[0228] After testing, the tap density of the above material reached 1.9g / cc, and the specific surface area of ​​the material was 8.8m 2 / g, the material's first discharge capacity in the half-cell voltage range of 2-4.8V reaches 257mAh / g, and the material's first coulombic efficiency in the half-cell reaches 88%. The compaction density of the positive electrode sheet prepared in step 8 is as high as 2.95 g / cc, and the first efficiency of the assembled full battery reaches 85%. In the full battery voltage range of 2~4.55V, the battery's energy density reaches 305Wh / Kg when discharged at 0.1C, and the full battery voltage range of 2.3~4.5V cycles 1400 cycles The capacity retention rate is 80%, and no gas is produced during the cycle, which is suitable for the basic needs of high-energy-density power battery applications.

[0229] Example 7

[0230] Precursor preparation:

[0231] A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and its application, comprising the following steps:

[0232] (1) preparing 50 L of 2 mol / L mixed salt solution 1 and 50 L of 2 mol / L mixed salt solution 2 by mixing nickel sulfate and manganese sulfate in a ratio of 1:1 and 1:3 respectively;

[0233] (2) adding the mixed salt solution 1 to the mixed salt solution 2 at a flow rate of 2 mL / min through a metering pump to obtain a mixed solution A;

[0234] (3) preparing 8 mol / L sodium hydroxide solution as a precipitant and 1.5 mol / L ammonia solution as a complexing agent;

[0235] (4) adding the mixed solution B at 3 mL / min, the complexing agent at 1.6 mL / min, and the precipitant at a certain speed into a coprecipitation reactor through a metering pump, controlling the reactor temperature at 48° C., the stirring speed at 450 r / min, and the reaction pH at about 10.9, and performing the coprecipitation reaction for 140 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0236] (5) Wash, filter and dry the above-mentioned material precursor suspension to obtain Ni 0.333 Mn 0.666 (OH)2 forms a nickel-cobalt-manganese multi-morphological manganese-rich hydroxide precursor; the precursor is a secondary spherical particle formed by stacking primary lamellar particles; the particle size D50 of the primary lamellar particles is 100nm; the particle size D50 of the secondary spherical particles is 20μm; the specific surface area of ​​the nickel-cobalt-manganese multi-morphological manganese-rich hydroxide precursor is 67m 2 / g;

[0237] Cathode material preparation:

[0238] (6) The above-mentioned single-component nickel-cobalt-manganese polymorphic manganese-rich hydroxide precursor contains Ni 0.333 Mn 0.666 (OH)2 and lithium carbonate are mixed in a solid phase according to a molar ratio of Li:Me=1.35 and sintered at a high temperature of 925°C for 16 hours to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material matrix oxide material;

[0239] (7) subjecting the above-mentioned single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material to surface modification treatment to obtain a single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material;

[0240] Positive electrode preparation:

[0241] (8) 95% by weight of the above-mentioned single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material is added together with 3.5% of conductive agent SP+carbon nanotubes (mass ratio of 6:1), 1.5% of binder PVDF, and solvent NMP, and added into a batching kettle and stirred to obtain a lithium-ion battery composite positive electrode material slurry;

[0242] (9) coating the single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material slurry on the positive electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the positive electrode material electrode sheet for standby use;

[0243] Negative electrode sheet preparation:

[0244] (10) Similarly, the negative electrode active material silicon-carbon composite negative electrode material (whose discharge capacity is 820 mAh / g), the conductive agent SP+carbon nanotubes (mass ratio is 2:1), the binder CMC, and the solvent SBR are mixed at a ratio of 93.5:1.5:1:4, and 70% of the solvent water is added into the batching kettle and stirred to obtain a lithium ion battery negative electrode material slurry;

[0245] (11) coating the negative electrode material slurry on the negative electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the negative electrode material electrode sheet for standby use;

[0246] Battery preparation:

[0247] (12) Assemble the above positive and negative electrode sheets into a 25Ah battery cell by lamination or winding;

[0248] (13) baking the battery cell, injecting electrolyte, and forming the battery cell to obtain a lithium-ion battery;

[0249] Performance Testing:

[0250] (14) The battery is charged to above 4.55 V for the first cycle and then activated and cycled within a voltage range of 2.3 to 4.5 V.

[0251] Test results:

[0252] After testing, the tap density of the above material reached 2.3g / cc, and the specific surface area of ​​the material was 2.8m 2 / g, the material's first discharge capacity in the half-cell voltage range of 2-4.8V reaches 267mAh / g, and the material's first coulombic efficiency in the half-cell reaches 88%. The compaction density of the positive electrode sheet prepared in step 8 is as high as 3.25 g / cc, and the first efficiency of the assembled full battery reaches 85%. In the full battery voltage range of 2~4.55V, the battery's energy density reaches 325Wh / Kg when discharged at 0.1C, and the full battery voltage range of 2.3~4.5V cycles 1500 cycles The capacity retention rate is 80%, and no gas is produced during the cycle, which is suitable for the basic needs of high-energy-density power battery applications.

[0253] Comparative Example 1

[0254] Precursor preparation:

[0255] A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and its application, comprising the following steps:

[0256] (1) preparing 100 L of a 2 mol / L mixed salt solution of nickel sulfate, cobalt sulfate and manganese sulfate in a ratio of 1:1:4;

[0257] (2) preparing a 2 mol / L sodium carbonate solution as a precipitant and a 0.8 mol / L ammonia solution as a complexing agent;

[0258] (3) adding the mixed salt solution through a metering pump at 3 mL / min, the complexing agent through a metering pump at 1 mL / min, and the precipitant through a metering pump at a certain speed into a coprecipitation reactor by controlling the reactor temperature at 56° C., the stirring speed at 750 r / min, and the reaction pH value at about 8.5, and performing the coprecipitation reaction for 45 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0259] (5) Wash, filter and dry the above-mentioned material precursor suspension to obtain Ni 0.167 Co 0.167 Mn 0.666 CO3 forms a nickel-cobalt-manganese manganese-rich carbonate precursor; the precursor is a secondary spherical particle formed by stacking primary lamellar particles; the particle size D50 of the primary lamellar particles is 200nm; the particle size D50 of the secondary spherical particles is 15.5μm; the specific surface area of ​​the nickel-cobalt-manganese manganese-rich carbonate precursor is 63m 2 / g;

[0260] Cathode material preparation:

[0261] (6) The above-mentioned single-component nickel-cobalt-manganese-rich manganese carbonate precursor contains Ni 0.167 Co 0.167 Mn 0.167 CO3 and lithium carbonate are mixed in a solid phase according to a molar ratio of Li:Me=1.45 and sintered at a high temperature of 850°C for 12 hours to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material matrix oxide material;

[0262] (7) subjecting the above-mentioned single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material to surface modification treatment to obtain a single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material;

[0263] Positive electrode preparation:

[0264] (8) 95% by weight of the above-mentioned single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material is added together with 3.5% of conductive agent SP+carbon nanotubes (mass ratio of 6:1), 1.5% of binder PVDF, and solvent NMP, and added into a batching kettle and stirred to obtain a lithium-ion battery composite positive electrode material slurry;

[0265] (9) coating the single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material slurry on the positive electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the positive electrode material electrode sheet for standby use;

[0266] Negative electrode sheet preparation:

[0267] (10) Similarly, a negative electrode active material silicon-carbon composite negative electrode material having a discharge capacity of 820 mAh / g, a conductive agent SP+carbon nanotubes (mass ratio of 2:1), a binder CMC, and a solvent SBR are mixed at a ratio of 93.5:1.5:1:4, and 70% of the total amount of solvent water is added into a batching kettle and stirred to obtain a lithium ion battery negative electrode material slurry;

[0268] (11) coating the negative electrode material slurry on the negative electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the negative electrode material electrode sheet for standby use;

[0269] Battery preparation:

[0270] (12) Assemble the above positive and negative electrode sheets into a 25Ah battery cell by lamination or winding;

[0271] (13) baking the battery cell, injecting electrolyte, and forming the battery cell to obtain a lithium-ion battery;

[0272] Performance Testing:

[0273] (14) The battery is charged to above 4.55 V for the first cycle and then activated and cycled within a voltage range of 2.3 to 4.5 V.

[0274] Test results:

[0275] After testing, the tap density of the above material reached 2.0 g / cc and the specific surface area of ​​the material was 7.95m 2 / g, the material's first discharge capacity in the half-cell voltage range of 2~4.8V reaches 300mAh / g, and the material's first coulombic efficiency in the half-cell reaches 92%. The compaction density of the positive electrode sheet prepared in step 8 is as high as 2.92 g / cc, and the first efficiency of the assembled full battery reaches 90%. In the full battery voltage range of 2~4.55V, the battery's energy density reaches 375Wh / Kg at 0.1C discharge, and the full battery voltage range of 2.3~4.5V cycles 800 cycles The capacity retention rate is 80%, and gas is produced during the cycle process, which cannot meet the basic application requirements of high-energy-density power batteries for long cycles.

[0276] Comparative Example 2

[0277] Precursor preparation:

[0278] A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material and its application, comprising the following steps:

[0279] (1) preparing 2 mol / L mixed salt solution 1 of 50 L, mixed salt solution 2 of 50 L, and mixed salt solution 3 of 50 L by mixing nickel sulfate, cobalt sulfate, and manganese sulfate in a ratio of 1:1:1, 1:1:4, and 1:1:7, respectively;

[0280] (2) preparing a 2 mol / L sodium carbonate solution as a precipitant and a 0.8 mol / L ammonia solution as a complexing agent;

[0281] (3) adding the mixed solution 1 through a metering pump at 3 mL / min, the complexing agent through a metering pump at 1 mL / min, and the precipitant through a metering pump at a certain speed into a coprecipitation reactor by controlling the reactor temperature at 56° C., the stirring speed at 750 r / min, and the reaction pH value at about 8.5, and performing the coprecipitation reaction for 15 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0282] (4) adding the mixed solution 2 at 3 mL / min, the complexing agent at 1 mL / min, and the precipitant at a certain speed into the coprecipitation reactor containing the nickel-cobalt-manganese carbonate suspension in the above step (3) through a metering pump, controlling the reactor temperature at 56° C., the stirring speed at 750 r / min, and the reaction pH at about 8.5, and performing the coprecipitation reaction for 15 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0283] (5) adding the mixed solution 3 through a metering pump at 3 mL / min, the complexing agent through a metering pump at 1 mL / min, and the precipitant through a metering pump at a certain speed to the coprecipitation reactor containing the nickel-cobalt-manganese carbonate suspension in step 4 above, and controlling the reactor temperature at 56° C., the stirring speed at 750 r / min, and the reaction pH at about 8.5, and performing the coprecipitation reaction for 15 hours to obtain a nickel-cobalt-manganese carbonate suspension;

[0284] (6) Wash, filter and dry the above-mentioned material precursor suspension to obtain Ni 0.167 Co 0.167 Mn 0.666 CO3 is used to form a nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor; the precursor is a secondary spherical particle formed by stacking primary lamellar particles; the particle size D50 of the primary lamellar particles is 200nm; the particle size D50 of the secondary spherical particles is 15.5μm; the specific surface area of ​​the nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor is 63m 2 / g;

[0285] Cathode material preparation:

[0286] (6) The above-mentioned single-component nickel-cobalt-manganese polymorphic manganese-rich carbonate precursor contains Ni 0.167 Co 0.167 Mn 0.167 CO3 and lithium carbonate are mixed in a solid phase according to a molar ratio of Li:Me=1.45 and sintered at a high temperature of 850°C for 12 hours to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material matrix oxide material;

[0287] (7) subjecting the above-mentioned single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material to surface modification treatment to obtain a single-composition polymorphic lithium-rich manganese-based positive electrode material matrix oxide material;

[0288] Positive electrode preparation:

[0289] (8) 95% by weight of the above-mentioned single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material is added together with 3.5% of conductive agent SP+carbon nanotubes (mass ratio of 6:1), 1.5% of binder PVDF, and solvent NMP, and added into a batching kettle and stirred to obtain a lithium-ion battery composite positive electrode material slurry;

[0290] (9) coating the single-composition multi-morphology lithium-rich manganese-based positive electrode material matrix oxide material slurry on the positive electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the positive electrode material electrode sheet for standby use;

[0291] Negative electrode sheet preparation:

[0292] (10) Similarly, the negative electrode active material silicon-carbon composite negative electrode material having a discharge capacity of 820 mAh / g, the conductive agent SP+carbon nanotubes (mass ratio of 2:1), the binder CMC, and the solvent SBR are mixed in a ratio of 93.5:1.5:1:4, and 70% of the total amount of solvent water is added into a batching kettle and stirred to obtain a lithium ion battery negative electrode material slurry;

[0293] (11) coating the negative electrode material slurry on the negative electrode current collector, drying the electrode sheet, slicing, and rolling to obtain the negative electrode material electrode sheet for standby use;

[0294] Battery preparation:

[0295] (12) Assemble the above positive and negative electrode sheets into a 25Ah battery cell by lamination or winding;

[0296] (13) baking the battery cell, injecting electrolyte, and forming the battery cell to obtain a lithium-ion battery;

[0297] Performance Testing:

[0298] (14) The battery is charged to above 4.55 V for the first cycle and then activated and cycled within a voltage range of 2.3 to 4.5 V.

[0299] Test results:

[0300] After testing, the tap density of the above material reached 1.98 g / cc and the specific surface area of ​​the material was 6.88m 2 / g, the material's first discharge capacity in the half-cell voltage range of 2~4.8V reaches 289mAh / g, and the material's first coulombic efficiency in the half-cell reaches 87%. The compaction density of the positive electrode sheet prepared in step 8 is as high as 2.92 g / cc, and the first efficiency of the assembled full battery reaches 88%. In the full battery voltage range of 2~4.55V, the battery's energy density reaches 345Wh / Kg at 0.1C discharge, and the full battery voltage range of 2.3~4.5V cycles 800 cycles The capacity retention rate is 82%, and there is a gas production problem during the cycle, which is suitable for the basic needs of high-energy-density power battery applications.

[0301] It can be seen from the above embodiments that the present invention provides a method for preparing a nickel-cobalt-manganese precursor, comprising the following steps: preparing a series of nickel-cobalt-manganese mixed salt solutions in different proportions, recorded as mixed salt solution 1, mixed salt solution 2, mixed salt solution 3 until mixed solution n; the manganese element concentration in mixed salt solution 1 → mixed salt solution n shows a gradient change trend; the mixed solution 1 is metered and pumped into the mixed salt solution 2 to obtain a mixed solution A; the mixed solution A is metered and pumped into the mixed salt solution 3 to obtain a mixed solution B; and the steps are performed successively until mixed with the mixed solution N to obtain a mixed solution; the mixed solution, the precipitant and the complexing agent are metered and pumped into a mixed manner, and then a coprecipitation reaction is carried out to obtain a nickel-cobalt-manganese precursor suspension; the nickel-cobalt-manganese precursor suspension is washed, filtered and dried to obtain a nickel-cobalt-manganese precursor. This method prepares a nickel-cobalt-manganese precursor with a high internal Mn content and a low surface Mn content, which is mixed with a lithium source in the solid phase for sintering, and then surface modified to obtain a single-composition multi-morphology lithium-rich manganese-based positive electrode material. Compared with traditional lithium-rich manganese-based positive electrode materials, the single-composition multi-morphology lithium-rich manganese-based positive electrode material has the same Mn content, so it can maintain a higher discharge capacity of the lithium-rich manganese-based positive electrode material. At the same time, it alleviates oxygen release during charging and greatly improves thermal stability. The first cycle efficiency of the full battery assembled with the positive electrode material prepared by this method reaches more than 85%; the energy density of the battery is between 305 and 380 Wh / Kg when the full battery is in the voltage range of 2~4.55V and 0.1C discharge; the full battery is cycled for at least 800 cycles in the voltage range of 2.3~4.5V, and the capacity retention rate is more than 80%; and no gas is produced during the cycle.

[0302] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a nickel-cobalt-manganese precursor, comprising the following steps: A series of nickel-cobalt-manganese mixed salt solutions with different proportions are prepared, which are recorded as mixed salt solution 1, mixed salt solution 2, mixed salt solution 3 to mixed solution n; the manganese element concentration in mixed salt solution 1 → mixed salt solution n shows a gradient change trend; The mixed solution 1 is metered and pumped into the mixed salt solution 2 to obtain a mixed solution A; The mixed solution A is metered and pumped into the mixed salt solution 3 to obtain a mixed solution B; and the process is repeated until it is mixed with the mixed solution N to obtain a mixed solution; The mixed solution, the precipitant and the complexing agent are mixed by metering pumping, and then coprecipitated to obtain a nickel-cobalt-manganese precursor suspension; the nickel-cobalt-manganese precursor suspension is washed, filtered and dried to obtain a nickel-cobalt-manganese precursor; The nickel-cobalt-manganese precursor has a composition of Formula 101, Formula 102 or Formula 103: Ni a0 Co b0 Mn c0 CO3 formula 101; Ni a0 Co b0 Mn c0 (OH)2 of Formula 102; Ni a0 Co b0 Mn c0 (COOH)2 formula 103; Among them, 0 <a0≤0.5,0≤b0<0.5,0.5≤c0<1。 2. The preparation method according to claim 1, characterized in that: The temperature of the coprecipitation reaction is 45~60°C; The coprecipitation reaction was carried out under stirring conditions with a stirring rate of 400-800 rpm; The pH value of the coprecipitation reaction is 7.5~11; The coprecipitation reaction time is 40~140h.

3. The preparation method according to claim 1, characterized in that: The precipitant is a water-soluble carbonate, a water-soluble acetate or a water-soluble hydroxide.

4. The preparation method according to claim 1, characterized in that: The nickel-cobalt-manganese precursor is a secondary spherical particle formed by stacking primary lamellar particles.

5. The preparation method according to claim 4, characterized in that: The particle size D50 of the primary sheet particles is 50-500 nm; The particle size D50 of the secondary spherical particles is 3 μm to 30 μm; The specific surface area of ​​the nickel-cobalt-manganese precursor is 1 to 85 m 2 / g.

6. A method for preparing a single-composition multi-morphological lithium-rich manganese-based positive electrode material, comprising the following steps: The nickel-cobalt-manganese precursor prepared by the preparation method according to any one of claims 1 to 5 is mixed with a lithium source in a solid phase and sintered to obtain Li d Ni x Co y Mn z O2; where d>1,0.1 <x<0.5,0<y<1,0.5≤z<1; Li d Ni x Co y Mn z O2 surface modification treatment to obtain a single-composition multi-morphological lithium-rich manganese-based positive electrode material; The single-composition multi-morphology lithium-rich manganese-based positive electrode material has a composition of Li d Ni a Co b Mn c O2;0 <a≤0.5,0≤b<0.5,0.5≤c<1。 7. The preparation method according to claim 6, characterized in that: The lithium-rich manganese-based positive electrode material is composed of the following substances composition: x1 Li d1 Ni a1 Co b1 Mn c1 O2, x2 Li d2 Ni a2 Co b2 Mn c2 O2, x3 Li d3 Ni a3 Co b3 Mn c3 O2, ······ xn Li dn Ni an Co bn Mn cn O2, where n ≥ 2; x1+ x2+ x3+…+ xn=1; a1+a2+a3+…+an=a; b1+b2+b3+…+bn=b; c1+c2+c3+……+cn=c; d1+d2+d3+……+dn=d.

8. A positive electrode sheet, prepared by coating a slurry made of a single-composition multi-morphological lithium-manganese-rich positive electrode material prepared by the preparation method according to any one of claims 6 to 7, a conductive agent, a binder and a solvent.

9. A lithium ion battery comprising the positive electrode sheet according to claim 8; and a negative electrode; The active material on the negative electrode plate is selected from one or more of graphite, artificial graphite, silicon-carbon material, lithium metal negative electrode and lithium-carbon negative electrode material.

Citation Information

Patent Citations

  • Lithium-ion-battery gradient cathode-material precursor and preparation method thereof

    CN104201369A

  • Lithium-rich positive electrode material and preparation method thereof

    CN104466158A

  • High-nickel gradient nickel cobalt manganese aluminum quaternary positive electrode material and preparation method thereof

    CN110518220A

  • Lithium-rich manganese-based lithium positive electrode material with full-concentration gradient distribution as well as preparation method and application thereof

    CN112624207A

  • Preparation of concentration gradient magnesium-doped lithium-rich manganese-based oxide positive electrode material and lithium battery application of concentration gradient magnesium-doped lithium-rich manganese-based oxide positive electrode material

    CN113299902A