Method for green synthesis of nano zero-valent iron modified biochar material and application of nano zero-valent iron modified biochar material
By loading nano-zero-valent iron on sludge biochar and using tea polyphenols as a reducing agent, the problem of efficient reduction of Cr(VI) in water was solved, achieving efficient removal of hexavalent chromium and reducing the agglomeration of nano-zero-valent iron. , demonstrating the environmental protection and economy of this method.
Patent Information
- Application Number
- CN202410729532.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing technology cannot effectively reduce hexavalent chromium (Cr(VI)) in water to less toxic trivalent chromium (Cr(III)), and nanoscale zero-valent iron is prone to agglomeration during the preparation and use process, resulting in its removal. Cr(VI) is not very effective.
Using tea polyphenols as a green reducing agent, the sludge is treated by hydrothermal carbonization to generate sludge biochar, and nano zero-valent iron is loaded onto the biochar. Combined with the antioxidant properties of tea polyphenols, the anti-oxidation properties of nano-zero-valent iron are improved. It has agglomeration and anti-oxidation properties, thereby effectively removing Cr(VI) from water.
It achieves the efficient reduction of Cr(Ⅵ) to Cr(Ⅲ), improves the removal capacity of sludge biochar, and reduces the agglomeration problem of nano zero-valent iron. Moreover, the method is simple to operate, low-cost, environmentally friendly, and suitable for high concentrations. Treatment of wastewater containing Cr(VI).
Smart Images

Figure CN118724236A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic nano material preparation and water purification environmental protection, and more specifically to a method for synthesizing nano zero-valent iron modified sludge biochar using tea polyphenols and a water treatment method. Background Art
[0002] Rapid urbanization and industrialization have inevitably led to serious heavy metal pollution, posing a serious threat to humans and the ecological environment. Chromium is a representative, highly toxic heavy metal element that is widely used in the electroplating industry, leather industry, and metal smelting industry. It enters water bodies due to improper disposal and improper discharge. The main forms of chromium are Cr(III) and Cr(VI). Cr(III) is a less toxic and more stable cation. It is one of the trace elements necessary for animals and plants and exists mainly in the form of sediments in water bodies. In contrast, Cr(VI) exists mainly in the form of oxygen-containing anions in water bodies. Long-term exposure to Cr(VI) can seriously harm the human immune system, reproductive system, and nervous system. It is one of the three typical carcinogenic heavy metals. Therefore, how to efficiently control and repair Cr(VI)-contaminated water bodies and ensure the quality of the water environment has become an important and realistic environmental problem that urgently needs to be studied and solved.
[0003] Biochar is the product of pyrolysis of biomass under oxygen-limited conditions. It has a large specific surface area and rich functional groups, and has been widely used to remove Cr(VI) from water. Previous data showed that China's rapid urbanization and industrialization have accelerated the development of the sewage treatment industry. A large amount of sludge has not been properly treated, and traditional sludge disposal methods (such as landfill, incineration and agricultural use) are facing increasing challenges. Hydrothermal carbonization technology does not require drying and grinding of wet sludge, and can convert materials with high moisture content into biochar at 180-240°C. Compared with the commonly used pyrolysis method (400-800°C) to prepare biochar, it has great potential in sludge reduction, harmlessness and resource treatment. Therefore, directly converting sludge into sludge biochar through hydrothermal carbonization to remove Cr(VI) from water bodies can not only reduce the risk of release of organic micropollutants and pathogen pollutants in sludge, realize the resource utilization of sludge, but also achieve the purpose of "waste treatment with waste". However, biochar cannot effectively reduce Cr(VI) to the less toxic Cr(III).
[0004] Studies have shown that nano-zero-valent iron is an environmentally friendly nanomaterial with strong reducing properties, which can efficiently remove Cr(VI). However, nano-zero-valent iron is prone to agglomeration and oxidation during preparation, transportation and use, and it is difficult to maintain a high level of electron transfer efficiency between it and pollutants. Therefore, using sludge biochar to load nano-zero-valent iron can not only effectively adsorb and reduce Cr(VI), but also improve the anti-agglomeration ability of nano-zero-valent iron, which is a win-win strategy. The commonly used method for synthesizing nano-zero-valent iron is chemical synthesis, which is to use expensive borohydride to convert Fe 2+ or Fe 3+ Reduction to Fe 0 However, due to the quantum tunneling effect and the mutual coupling of interface atoms, the synthesized nano-zero-valent iron is easy to agglomerate into a chain structure or a cluster structure, resulting in an increase in particle size and a decrease in specific surface area.
[0005] Compared with the use of borohydrides, plant extracts (such as tea polyphenols) have the advantages of low cost and environmental protection, and are widely used in the preparation of nano zero-valent iron. However, the effect of using tea polyphenols to reduce Cr (VI) is affected by factors such as the amount of tea polyphenols added, reaction temperature and reaction time.
[0006] Therefore, how to use tea polyphenols as a green reducing agent to prepare nano zero-valent iron with significant antioxidant properties is an urgent problem that technicians in this field need to solve. Summary of the invention
[0007] In terms of efficient control and restoration of Cr(VI)-contaminated water bodies, biochar cannot effectively reduce Cr(VI) to less toxic Cr(III). The commonly used biochar modification method is to load nano-zero-valent iron. However, due to the quantum tunneling effect and the mutual coupling of interface atoms, the synthesized nano-zero-valent iron is easy to agglomerate into a chain structure or cluster structure, resulting in an increase in particle size, a decrease in specific surface area, a poor reduction effect on Cr(VI), and difficulty in preservation.
[0008] In view of this, the present invention provides a green synthetic nano zero-valent iron modified biochar material for removing Cr(VI) from water bodies, which can efficiently control and repair Cr(VI)-contaminated water bodies.
[0009] In order to achieve the above object, the present invention provides a method for green synthesis of nano zero-valent iron modified biochar material, comprising the following steps:
[0010] Step 1: Obtain raw materials, obtain wet sludge obtained from the sewage treatment plant through filter pressing and dehydration process;
[0011] Step 2: Stone removal: preliminary screening of wet sludge to remove stones and other impurities;
[0012] Step 3: hydrothermal carbonization, using a hydrothermal synthesis reactor for hydrothermal carbonization;
[0013] Step 4: solid-liquid separation. After the reaction is completed, cool to room temperature and filter the mixed solution through a 0.45 μm water filter membrane to obtain a solid product.
[0014] Step 5: Drying: placing the obtained solid product in a forced air drying oven to dry;
[0015] Step 6: Grind through a 60-mesh sieve to obtain sludge biochar;
[0016] Step 7: preparing Fe(II) solution;
[0017] Step 8: Add sludge biochar to the Fe(Ⅱ) solution and stir evenly;
[0018] Step 9: Continue to add tea polyphenols and stir evenly;
[0019] Step 10: Solid-liquid separation: after the reaction is completed, cool to room temperature and filter using a 0.45 μm water filter membrane to obtain a solid product;
[0020] Step 11: Drying: placing the obtained solid product in a forced air drying oven to dry;
[0021] Step 12: Grind through a 60-mesh sieve;
[0022] Step 13: Finished product packaging: Use a sealing machine to package the sieved finished products.
[0023] Preferably, in the first step, the moisture content of the wet sludge is 60% to 85%.
[0024] The beneficial effects of adopting the above-mentioned moisture content are: the method is relatively simple, and the wet sludge produced by the sewage treatment plant can be directly used. Compared with the pyrolysis method, there is no need to dry the sludge, which is simpler and more energy-saving.
[0025] Preferably, in the third step, the wet sludge and water are subjected to hydrothermal carbonization, and the ratio of the wet sludge to water is 0.6-0.8; the reaction temperature of the hydrothermal carbonization is 200-240° C., and the reaction time is 2 hours.
[0026] The beneficial effects of adopting the above hydrothermal conditions are:
[0027] Wet sludge itself contains a certain amount of water. When mixed with water in a certain proportion, the hydrothermal carbonization effect is better. According to the experimental results, at 200-240℃, hydrothermal carbonization for two hours can produce the largest specific surface area and the strongest adsorption capacity of sludge biochar.
[0028] Preferably, in the fifth step, the drying is performed at 100-120° C. for 8-12 hours.
[0029] Furthermore, in the seventh step, the specific operation of preparing the Fe(II) solution is as follows:
[0030] Add 10.0-25.0g FeSO4·7H2O (containing 2.0-5.0gFe 2+ ), use a magnetic stirrer, at 20-30°C, 500-800 r / min, and stir for 0.5 h.
[0031] Preferably, in the eighth step, the amount of sludge biochar added is 10.0-25.0 g / L; and the stirring is performed at 25-30° C. and 500-800 r / min for 0.5-1.5 h.
[0032] Preferably, in the ninth step, the amount of tea polyphenols added is 10.0-30.0 g / L; and the stirring is carried out at 70-80° C. and 500-800 r / min for 2-3 hours.
[0033] The beneficial effects of adopting the above technical solution are:
[0034] The commonly used method for preparing nano zero-valent iron is the borohydride reduction method. However, the use of borohydride to prepare nano zero-valent iron needs to be carried out in a nitrogen environment, and the prepared nano zero-valent iron is easily oxidized and cannot maintain its reducing ability for a long time. Tea polyphenols, as a green reducing agent, have strong antioxidant properties. The use of tea polyphenols as a reducing agent to prepare nano zero-valent iron does not require a nitrogen environment and can maintain a strong reducing ability for a long time. Therefore, tea polyphenols are used to prepare nano zero-valent iron.
[0035] Preferably, in the eleventh step, the drying is performed at 60-70° C. for 8-12 hours.
[0036] It can be seen from the above technical solutions that, compared with the prior art, the technical effects achieved by the present invention are:
[0037] The sludge generated during sewage treatment is recycled into biochar and applied to the removal of Cr(VI) in wastewater. This can not only control the secondary pollution that may be caused by sludge from the source, but also achieve the purpose of "treating waste with waste". Nano-zero-valent iron has low cost, large specific surface area, high activity, and strong reducing ability, and can effectively reduce Cr(VI) to Cr(III). Loading nano-zero-valent iron onto sludge biochar not only solves the problem of easy agglomeration of nano-zero-valent iron, but also improves the ability of sludge biochar to remove Cr(VI). The green reducing agent tea polyphenols extracted from green tea are used to synthesize nano-zero-valent iron, which can further improve the anti-agglomeration and antioxidant properties of nano-zero-valent iron.
[0038] Based on the above situation, the present invention proposes a method for preparing a green synthetic nano zero-valent iron modified sludge biochar composite material using tea polyphenols as a reducing agent and sludge biochar as a supporting material. The method is simple to operate, low in cost, and green and environmentally friendly.
[0039] The composite material prepared by this method can effectively treat high-concentration Cr(VI)-containing wastewater. When the initial Cr(VI) concentration is 50.0 mg / L, the initial solution pH is 7, the reaction temperature is 25°C, and the composite material dosage is 1 g / L, the removal amount of hexavalent chromium reaches 23.0 mg / g. It has broad application prospects in the field of treating Cr(VI)-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0041] Figure 1 This is a scanning electron microscope image of the green synthesis of nano-zero-valent iron modified sludge biochar composite material.
[0042] Figure 2 This is the X-ray diffraction pattern of the green synthesized nano zero-valent iron modified sludge biochar composite material.
[0043] Figure 3 This is a comparison chart of the experimental results of removing Cr(VI) by sludge biochar and green synthetic nano zero-valent iron modified sludge biochar composite material.
[0044] Figure 4 The figure is a diagram showing the removal effect of Cr(VI) in water by the composite material prepared by the present invention at different initial pH values.
[0045] Figure 5 The figure is a diagram showing the removal effect of Cr(VI) in water by the composite material prepared by the present invention at different dosages.
[0046] Figure 6 The figure is a diagram showing the removal effect of Cr(VI) in water by the composite material prepared by the present invention under different regeneration cycles. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] The sludge generated during sewage treatment is recycled into biochar and applied to the removal of Cr(VI) in wastewater, which can not only control the secondary pollution caused by sludge from the source, but also achieve the purpose of "waste treatment with waste". However, sludge biochar only has an adsorption effect on Cr(VI) and cannot effectively reduce Cr(VI) to Cr(III). Nano-zero-valent iron has low cost, large specific surface area, high activity and strong reducing ability, and can effectively reduce Cr(VI) to Cr(III). However, the problem of easy agglomeration and oxidation of nano-zero-valent iron limits its application. Loading nano-zero-valent iron on sludge biochar not only solves the problem of easy agglomeration of nano-zero-valent iron, but also improves the ability of sludge biochar to remove Cr(VI). The synthesis of nano-zero-valent iron using tea polyphenols, a green reducing agent extracted from plants, can further improve the anti-agglomeration and antioxidant properties of nano-zero-valent iron. However, the effect of nano-zero-valent iron prepared by tea polyphenols on reducing Cr(VI) is affected by factors such as the amount of tea polyphenols added, reaction temperature and reaction time. Based on the above situation, the present invention uses tea polyphenols as a reducing agent and sludge biochar as a supporting material, optimizes the preparation conditions through experiments, and prepares a modified composite material.
[0049] Embodiment 1:
[0050] A preparation process of nano zero-valent iron modified sludge biochar, comprising the following processing steps:
[0051] Step 1: Obtain raw materials, obtain wet sludge (water content 75%) obtained by filter pressing and dehydration process from a sewage treatment plant;
[0052] Step 2: Stone removal: preliminary screening of the wet sludge to remove various impurities such as stones;
[0053] Step 3: Hydrothermal carbonization, using a hydrothermal synthesis reactor for hydrothermal carbonization. Put wet sludge and water into the hydrothermal carbonization reactor, with a sludge to water ratio of 0.7. Then use a blast drying oven to heat the hydrothermal synthesis reactor to 220°C and keep it at this temperature for 2 hours;
[0054] Step 4: Solid-liquid separation: move the hydrothermal synthesis reactor after the reaction to a ventilated place, wait for it to cool to room temperature, open the reactor, pour the mixed solution after the reaction into a beaker, and use a 0.45μm water filter membrane to separate the liquid and the solid;
[0055] Step 5: Drying: placing the obtained solid product in a forced air drying oven and drying at 110°C for 12 hours;
[0056] Step 6: Grind and sieve: Grind the dried solid product and pass it through a 60-mesh sieve;
[0057] Step 7: Prepare Fe(Ⅱ) solution by adding 15.0g FeSO4·7H2O (containing 3.0g Fe 2+ ), using a magnetic stirrer, stir at 25°C and 600 r / min for 0.5 h to completely dissolve;
[0058] Step 8: Add sludge biochar, add 2.0g sludge biochar to every 1L water, continue to use the magnetic stirrer, stir for 1h at 25℃ and 600r / min;
[0059] Step 9: Add tea polyphenols. Continue to add 20.0 g of tea polyphenols to every 1 L of water, and then use a magnetic stirrer to stir for 2.5 h at 75.0 ° C and 600 r / min;
[0060] Step 10: Solid-liquid separation: after the reaction is completed, wait for it to cool to room temperature, pour the mixed solution after the reaction into a beaker, and use a 0.45 μm water filter membrane to separate the liquid and the solid;
[0061] Step 11: Drying: placing the obtained solid product in a forced air drying oven and drying at 65°C for 12h;
[0062] Step 12: Grind and sieve: Grind the dried solid product and pass it through a 60-mesh sieve;
[0063] Step 13: Finished product packaging: Use a sealing machine to package the sieved finished products.
[0064] The composite materials prepared under the above conditions were characterized.
[0065] The scanning electron microscope image is as follows Figure 1 As shown in the figure, a large number of nano zero-valent iron particles with a diameter of 100 to 200 nm are formed during the preparation of the composite material. These spherical nano zero-valent iron particles are similar in size, shape and uniformly distributed, which greatly increases the adsorption sites of the composite material.
[0066] Its X-ray diffraction image is as follows Figure 2 As shown, the composite material was analyzed by X-ray diffraction (XRD). There is an obvious SiO2 diffraction peak in the XRD spectrum of the sludge biochar, which is consistent with the presence of SiO2 in the sludge biochar. The XRD spectrum of the composite material lacks an obvious diffraction peak at 2θ = 45°, which is due to the Fe 0The diffraction peaks of green synthesized nano-zero-valent iron show an amorphous structure. The broad diffraction peak at 2θ=20° can be considered as an organic substance with TP as a reducing agent, but the diffraction peak signal is weak, which may be due to being covered by the SiO2 peak.
[0067] Embodiment 2:
[0068] A preparation process of nano zero-valent iron modified sludge biochar, comprising the following processing steps:
[0069] Step 1: Obtain raw materials, obtain wet sludge (water content 85%) obtained by filter pressing and dehydration process from a sewage treatment plant;
[0070] Step 2: Stone removal: preliminary screening of the wet sludge to remove various impurities such as stones;
[0071] Step 3: Hydrothermal carbonization, using a hydrothermal synthesis reactor for hydrothermal carbonization. Put wet sludge and water into the hydrothermal carbonization reactor, with a sludge to water ratio of 0.8. Then use a blast drying oven to heat the hydrothermal synthesis reactor to 240°C and keep it at this temperature for 2 hours;
[0072] Step 4: Solid-liquid separation: move the hydrothermal synthesis reactor after the reaction to a ventilated place, wait for it to cool to room temperature, open the reactor, pour the mixed solution after the reaction into a beaker, and use a 0.45μm water filter membrane to separate the liquid and the solid;
[0073] Step 5: Drying: placing the obtained solid product in a forced air drying oven and drying at 120°C for 12h;
[0074] Step 6: Grind and sieve: Grind the dried solid product and pass it through a 60-mesh sieve;
[0075] Step 7: Prepare Fe(Ⅱ) solution by adding 25.0g FeSO4·7H2O (containing 5.0g Fe 2+ ), using a magnetic stirrer, stir at 30°C and 800 r / min for 0.5 h to completely dissolve;
[0076] Step 8: Add sludge biochar, add 5.0g sludge biochar to every 1L water, continue to use the magnetic stirrer, stir at 30℃ and 800r / min for 1.5h;
[0077] Step 9: Add tea polyphenols, add 30.0g of tea polyphenols to every 1L of water, and then use a magnetic stirrer to stir for 3.0h at 80.0℃ and 800r / min;
[0078] Step 10: Solid-liquid separation: after the reaction is completed, wait for it to cool to room temperature, pour the mixed solution after the reaction into a beaker, and use a 0.45 μm water filter membrane to separate the liquid and the solid;
[0079] Step 11: Drying: placing the obtained solid product in a forced air drying oven and drying at 70.0°C for 12h;
[0080] Step 12: Grind and sieve: Grind the dried solid product and pass it through a 60-mesh sieve;
[0081] Step 13: Finished product packaging: Use a sealing machine to package the sieved finished products.
[0082] Embodiment three:
[0083] A preparation process of nano zero-valent iron modified sludge biochar, comprising the following processing steps:
[0084] Step 1: Obtain raw materials, obtain wet sludge (water content 65%) obtained by filter pressing and dehydration process from a sewage treatment plant;
[0085] Step 2: Stone removal: preliminary screening of the wet sludge to remove various impurities such as stones;
[0086] Step 3: Hydrothermal carbonization, using a hydrothermal synthesis reactor for hydrothermal carbonization. Put wet sludge and water into the hydrothermal carbonization reactor, with a sludge to water ratio of 0.6. Then use a blast drying oven to heat the hydrothermal synthesis reactor to 200°C and keep it at this temperature for 2 hours;
[0087] Step 4: Solid-liquid separation: move the hydrothermal synthesis reactor after the reaction to a ventilated place, wait for it to cool to room temperature, open the reactor, pour the mixed solution after the reaction into a beaker, and use a 0.45μm water filter membrane to separate the liquid and the solid;
[0088] Step 5: Drying: placing the obtained solid product in a forced air drying oven and drying at 100°C for 8 hours;
[0089] Step 6: Grind and sieve: Grind the dried solid product and pass it through a 60-mesh sieve;
[0090] Step 7: Prepare Fe(Ⅱ) solution by adding 10.0g FeSO4·7H2O (containing 2.0g Fe 2+ ), using a magnetic stirrer, stir at 20°C and 500 r / min for 0.5 h to completely dissolve;
[0091] Step 8: Add sludge biochar, add 1.0g sludge biochar to every 1L water, continue to use the magnetic stirrer, stir at 20℃, 500r / min, for 0.5h;
[0092] Step 9: Add tea polyphenols. Continue to add 10.0 g of tea polyphenols to every 1 L of water, and then use a magnetic stirrer to stir for 2.0 h at 70.0 ° C and 500 r / min;
[0093] Step 10: Solid-liquid separation: after the reaction is completed, wait for it to cool to room temperature, pour the mixed solution after the reaction into a beaker, and use a 0.45 μm water filter membrane to separate the liquid and the solid;
[0094] Step 11: Drying: placing the obtained solid product in a forced air drying oven and drying at 60°C for 8h;
[0095] Step 12: Grind and sieve: Grind the dried solid product and pass it through a 60-mesh sieve;
[0096] Step 13: Finished product packaging: Use a sealing machine to package the sieved finished products.
[0097] Embodiment 4:
[0098] The composite material prepared in Example 1 was used for the experiment. 0.03 g of the corresponding adsorbent (sludge biochar or composite material) was accurately weighed and transferred to a centrifuge tube. Then, 30 mL of a 50 mg / L Cr(VI) solution with a pH value of 7 was injected into the centrifuge tube (i.e., the adsorbent dosage was 1 g / L). Then, the centrifuge tube was continuously oscillated at 180 rpm and 25 ° C using an air bath thermostatic oscillator. Samples were taken from the reaction mixture at predetermined time intervals (0.083, 0.167, 0.5, 1, 2, 4, 8, 12, 16, 20 and 24 h) and filtered with a 0.45 μm filter membrane. The absorbance was measured at a wavelength of 540 nm using a UV-visible spectrophotometer to calculate the concentration of Cr(VI) in the filtrate.
[0099] The experimental results are as follows Figure 3 As shown in the figure, the adsorption of Cr(VI) by the composite material reaches adsorption equilibrium within 16 hours, and the removal capacity of the composite material for Cr(VI) reaches 23.0 mg / g, while the removal capacity of Cr(VI) by sludge biochar is only 2.7 mg / g. The removal capacity of the composite material for Cr(VI) is significantly better than that of sludge biochar. This is mainly due to the presence of a large amount of nano zero-valent iron on the surface of the composite material. In the initial stage of adsorption, a large amount of nano zero-valent iron on the surface of the composite material has a strong reducing ability for Cr(VI), so the initial adsorption rate is fast. As the reaction process proceeds, the unreacted nano zero-valent iron gradually decreases, the reaction rate decreases, and the reaction enters a state of equilibrium.
[0100] Embodiment five:
[0101] The composite material prepared in Example 1 was used for the experiment. 30 mL of Cr(VI) solution with an initial concentration of 50 mg / L was transferred to each centrifuge tube, and the pH was adjusted to 2, 3, 4, 5, 6, 7, 8, 9, and 10, respectively. 0.03 g of the green synthetic nano zero-valent iron modified sludge biochar composite material prepared by the present invention was added to the centrifuge tube, and it was placed in a constant temperature oscillation box at 25°C and shaken at 180 r / min for 16.0 h. After the experiment, the supernatant was taken after static precipitation, and the concentration of Cr(VI) was determined by diphenylcarbonyl disulfide spectrophotometry to obtain the removal effect diagram of Cr(VI) of the material at different pH values. It can be seen from this that the present invention uses tea polyphenols to green synthesize nano zero-valent iron modified sludge biochar composite materials, and has a good removal effect on Cr(VI) under different conditions. The material can effectively remove Cr(VI) from water bodies.
[0102] The experimental results are as follows Figure 4 As shown in the figure, the removal effect of the composite material on Cr(VI) is significantly better under acidic conditions, indicating that low pH is conducive to the removal of Cr(VI), which may be related to the existence form of Cr(VI) in the solution. When the pH of the solution is less than 6, the Cr(VI) in the solution is mainly in the form of HCrO4 - Exists in the form of ions, HCrO4 - The oxidation capacity is higher than CrO4 2- . Under lower solution pH conditions, the electron transfer ability between the composite material and Cr(VI) is stronger. The process of reducing Cr(VI) by nano zero-valent iron is an acid-driven surface-mediated process. Acidic conditions are conducive to the decomposition of the surface passivation layer and the corrosion of nano zero-valent iron, as well as the elimination of hydroxide precipitation on the surface of the composite material. At a pH of 2.0, the composite material's ability to remove Cr(VI) can reach 50 mg / g. On the contrary, under alkaline conditions, hydroxide (such as Fe(OH)3, Cr(OH)3, etc.) precipitation is easily formed. If the precipitate is adsorbed on the surface of the composite material, the surface of the nano zero-valent iron will be passivated and the reaction activity will be reduced. This shows that the lower the solution pH, the more conducive it is to the removal of Cr(VI) by the composite material.
[0103] Embodiment six:
[0104] The composite material prepared in Example 1 was used for the experiment. 30 mL of Cr(VI) solution with an initial concentration of 50 mg / L and a pH of 7 was transferred to each centrifuge tube. 0.015 g, 0.03 g, 0.045 g, 0.06 g, and 0.09 g of the green synthetic nano zero-valent iron modified sludge biochar composite material prepared by the present invention were added to the centrifuge tubes respectively, and the composite material was placed in a constant temperature oscillation box at 25 ° C and shaken at 180 r / min for 16.0 h. After the experiment, the supernatant was taken after static precipitation, and the concentration of Cr(VI) was determined by diphenylcarbonyl disulfide spectrophotometry to obtain the removal effect diagram of Cr(VI) at different dosages of the material. It can be seen from this that the present invention uses tea polyphenols to green synthesize nano zero-valent iron modified sludge biochar composite materials. As its dosage increases from 0.5 g / L to 3 g / L, the Cr(VI) removal rate increases from 48.59% to 99.99%, and the removal effect is good.
[0105] The experimental results are as follows Figure 5 As shown in the figure, as the dosage of the composite material increases from 0.5 g / L to 3 g / L, the Cr(VI) removal rate increases from 48.59% to 99.99%, while the unit adsorption capacity of the composite material decreases from 48.59 mg / g to 16.86 mg / g. This is mainly due to the relatively limited adsorption sites on its surface when the dosage of the composite material is low, resulting in low removal efficiency. In contrast, a higher dosage can provide more adsorption sites, thereby improving the removal efficiency. However, excessive amounts of composite materials can lead to an increase in the agglomeration of the adsorbent particles, resulting in a decrease in the total surface area of the composite material and a decrease in the adsorption capacity per unit of the composite material.
[0106] Embodiment seven:
[0107] The composite material prepared in Example 1 was used for the experiment. 30 mL of Cr(VI) solution with an initial concentration of 50 mg / L and a pH of 7 was transferred to each centrifuge tube. 0.03 g of the green synthetic nano zero-valent iron modified sludge biochar composite material prepared by the present invention was added to each centrifuge tube, and it was placed in a constant temperature oscillating box at 25°C and shaken at 180 r / min for 16.0 h. After the experiment, the precipitation was allowed to stand, the composite material was separated, and it was soaked in 0.1 mol / L HCl at room temperature for 1 h, and then filtered using a 0.45 μm water filter membrane to separate the liquid and the solid; the obtained solid product was placed in a blast drying oven and dried at 65°C for 12 h to obtain a regenerated composite material. After each adsorption was completed, the supernatant was taken and the concentration of Cr(VI) was determined by diphenylcarbonyl disulfide spectrophotometry. The process was repeated 5 times. The removal effect diagram of Cr(VI) of the material under different regeneration cycles was obtained.
[0108] The experimental results are as follows Figure 6As shown in Figure 2, in this study, the composite material after adsorption of Cr(VI) was collected by filtration and the Cr(III) and Fe(III) oxide layers were regenerated by dissolving them with hydrochloric acid solution. After the first adsorption / desorption cycle, the removal capacity of the composite material for Cr(VI) did not decrease significantly. After 5 cycles, the q of the composite material for Cr(VI) was e The content of the composite material can still reach 11.28 mg / g. This result shows that the composite material prepared by the present invention has good reusability and good practical application prospects.
[0109] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for green synthesis of nano zero-valent iron modified biochar material, characterized in that: The steps include: Step 1: Obtain raw materials, obtain wet sludge obtained from the sewage treatment plant through filter pressing and dehydration process; Step 2: Stone removal: preliminary screening of wet sludge to remove stones and other impurities; Step 3: hydrothermal carbonization, using a hydrothermal synthesis reactor for hydrothermal carbonization; Step 4: solid-liquid separation. After the reaction is completed, cool to room temperature and filter the mixed solution through a 0.45 μm water filter membrane to obtain a solid product. Step 5: Drying; Step 6: Grind through a 60-mesh sieve to obtain sludge biochar; Step 7: preparing Fe(II) solution; Step 8: Add sludge biochar to the Fe(Ⅱ) solution and stir evenly; Step 9: Continue to add tea polyphenols and stir evenly; Step 10: Solid-liquid separation: after the reaction is completed, cool to room temperature and filter using a 0.45 μm water filter membrane to obtain a solid product; Step 11: Drying; Step 12: Grind through a 60-mesh sieve; Step 13: Finished product packaging.
2. The method for green synthesis of nano zero-valent iron modified biochar material according to claim 1, characterized in that: In the first step, the moisture content of the wet sludge is 60% to 85%.
3. The method for green synthesis of nano zero-valent iron modified biochar material according to claim 1, characterized in that: In the third step, the wet sludge and water are subjected to hydrothermal carbonization, and the ratio of the wet sludge to water is 0.6-0.8; the reaction temperature of the hydrothermal carbonization is 200-240° C., and the reaction time is 2 hours.
4. The method for green synthesis of nano zero-valent iron modified biochar material according to claim 1, characterized in that: In the fifth step, the drying is performed at 100-120° C. for 8-12 hours.
5. The method for green synthesis of nano zero-valent iron modified biochar material according to claim 1, characterized in that: In the seventh step, the specific operation of preparing the Fe(II) solution is: Add 10.0-25.0 g of FeSO4·7H2O to every 1 L of water and stir for 0.5 h at 20-30°C and 500-800 r / min.
6. The method for green synthesis of nano zero-valent iron modified biochar material according to claim 1, characterized in that: In the eighth step, the amount of the sludge biochar added is 10.0-25.0 g / L; the stirring is carried out at 25-30° C. and 500-800 r / min for 0.5-1.5 h.
7. The method for green synthesis of nano zero-valent iron modified biochar material according to claim 1, characterized in that: In the ninth step, the amount of tea polyphenols added is 10.0-30.0 g / L; the stirring is carried out at 70-80° C. and 500-800 r / min for 2-3 hours.
8. The method for green synthesis of nano zero-valent iron modified biochar material according to claim 1, characterized in that: In the eleventh step, the drying is performed at 60-70° C. for 8-12 hours.
9. An application of green synthetic nano zero-valent iron modified biochar material, characterized in that: Application of nano zero-valent iron modified biochar material prepared by the method as described in any one of claims 1-8 in removing Cr(VI) from water.
Citation Information
Patent Citations
Preparation and application of greenly synthesized biochar supported zero-valent iron nanomaterial
CN108043361A
Method for remedying acidified arsenic contaminated soil by biochar-loaded nano-scale zero-valent iron cooperated with bacteria
CN109570227A
Cited By
Zero-valent iron protection catalytic membrane as well as preparation method and application thereof
CN120618528A