Glass ceramic as well as preparation method and application thereof

By preparing glass-ceramics with a specific formula, the problems of insufficient strength and difficulty in processing of existing glass-ceramics are solved, and the properties of scratch resistance, drop resistance and easy processing are achieved. It is suitable for smart watch structural parts, providing transparency and Aesthetic effect.

CN118724465APending Publication Date: 2024-10-01BEIJING XIAOMI MOBILE SOFTWARE CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310334655.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing glass-ceramics lack strength, are prone to scratches on the surface, and are difficult to process, making them unable to meet the performance requirements of smart watch structural parts.

Method used

Adopting a glass-ceramic formula, containing 40-60% SiO2, 2-18% Al2O3, 6-22% B2O3, 2-8% SrO, 2-8% SnO2, 5-15% ZnO , 0.1~10% B i2O3, 0~12% MgO, 0~12% CaO, 0.1~10% Li2O and 0~20% ZrO2 are prepared by ball milling, melting, annealing, nucleation, crystallization and salt bath treatment to increase glass stability and crystallization ability.

Benefits of technology

It achieves anti-scratch, anti-drop, and easy-to-process properties, and is suitable for smart watch structural parts, providing transparent effects and enriching aesthetic effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention relates to microcrystalline glass as well as a preparation method and application thereof. The microcrystalline glass is prepared from 40 to 60 weight percent of SiO2, 2 to 18 weight percent of Al2O3, 6 to 22 weight percent of B2O3, 2 to 8 weight percent of SrO, 2 to 8 weight percent of SnO2, 5 to 15 weight percent of ZnO, 0.1 to 10 weight percent of Bi2O3, 0 to 12 weight percent of MgO, 0 to 12 weight percent of CaO, 0.1 to 10 weight percent of Li2O, 0 to 18 weight percent of TiO2 and 0 to 20 weight percent of ZrO2. Wherein the microcrystalline glass comprises at least one component selected from the group consisting of MgO and CaO, and at least one component selected from the group consisting of TiO2 and ZrO2. The microcrystalline glass disclosed by the invention has the properties of scratch resistance, drop resistance and easiness in processing, can realize a transparent effect when being applied to a shell, and can enrich the attractive effect of the shell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of microcrystalline glass, and in particular, to a microcrystalline glass and a preparation method and application thereof. Background Art

[0002] Wearable devices must not only meet the user's inherent need for beauty, but also fully consider the impact of materials on skin health. Currently, the appearance and structural parts of smart watches include the middle frame, back shell, strap and watch dial. Among them, the materials of the middle frame are mostly stainless steel, titanium alloy, aluminum alloy, ceramic, etc., the materials of the back shell are mostly plastic, ceramic, sapphire, etc., the materials of the strap are mostly leather, silicone, TPU, ceramic, metal, etc., and the materials of the watch dial are mostly random glass, microcrystalline glass, sapphire, etc.

[0003] In the prior art, the middle frame, strap and back shell are mostly achieved with the help of masterbatch, spraying, PVD, anodizing and other methods to achieve different appearance colors. Due to the insufficient tightness between the material and the coating, the coating has fallen off; the color of the aluminum alloy anode is relatively monotonous and has potential health hazards. In contrast, glass is more skin-friendly than plastic and silicone; the density is lower than stainless steel and ceramics; the color is richer than ceramics, metals and plastics. In addition, after the glass is microcrystallized, it not only retains the characteristics of the glass itself, but also makes its physical properties close to ceramics. However, due to the insufficient strength of the microcrystalline glass in the prior art, scratches are easily found on the surface, and it is difficult to process. Summary of the invention

[0004] The purpose of the present disclosure is to provide a microcrystalline glass that is scratch-resistant, easy to process, and can meet the performance requirements of watch structural parts.

[0005] In order to achieve the above-mentioned purpose, the first aspect of the present disclosure provides a microcrystalline glass, which contains, based on the total weight of the microcrystalline glass, 40 to 60 weight % of SiO2, 2 to 18 weight % of Al2O3, 6 to 22 weight % of B2O3, 2 to 8 weight % of SrO, 2 to 8 weight % of SnO2, 5 to 15 weight % of ZnO, 0.1 to 10 weight % of Bi2O3, 0 to 12 weight % of MgO, 0 to 12 weight % of CaO, 0.1 to 10 weight % of Li2O, 0 to 18 weight % of TiO2 and 0 to 20 weight % of ZrO2; wherein the microcrystalline glass includes at least one component of MgO and CaO, and at least one component of TiO2 and ZrO2.

[0006] Optionally, based on the total weight of the microcrystalline glass, the microcrystalline glass contains: 40 to 56 weight % SiO2, 2 to 15 weight % Al2O3, 8 to 20 weight % B2O3, 2 to 8 weight % SrO, 2 to 8 weight % SnO2, 5 to 10 weight % ZnO, 0.1 to 10 weight % Bi2O3, 0 to 12 weight % MgO, 0 to 10 weight % CaO, 0.1 to 10 weight % Li2O, 0 to 15 weight % TiO2 and 0 to 15 weight % ZrO2.

[0007] Optionally, in the microcrystalline glass, the ratio of the total mass of SiO2 and B2O3 to the total mass of Li2O and Na2O is 10 to 65, the ratio of the total mass of SrO and SnO2 to the mass of ZnO is 0.4 to 1.5, the ratio of the total mass of ZnO and Al2O3 to the mass of Li2O is 4 to 30, and the ratio of the total mass of TiO2 and ZrO2 to the mass of Li2O is 2 to 27.

[0008] Optionally, based on the total weight of the glass-ceramics, the glass-ceramics further contains no more than 6 weight % of Na2O.

[0009] Optionally, the glass-ceramic further contains coloring ions, wherein the coloring ions are selected from Cu 2+ , Fe 3+ 、Ni 4+ , Mn 4+ and Co 4+ At least one of .

[0010] Optionally, the microcrystalline glass also contains a coloring oxide, and the coloring oxide is selected from at least one of CuO, Fe2O3, NiO2, MnO2 and CoO2; based on the total weight of the microcrystalline glass, the microcrystalline glass contains: 0 to 2 weight % CuO, 0 to 5 weight % Fe2O3, 0 to 3 weight % NiO2, 0 to 3 weight % MnO2, and 0 to 2 weight % CoO2.

[0011] Optionally, the crystallization degree of the microcrystalline glass is 50-95%; the grain size range is 10-100 nm; when the thickness of the microcrystalline glass is 0.5 mm, the visible light transmittance range is 20-85%.

[0012] Optionally, the crystal phase in the glass-ceramics includes at least one of a spodumene crystal phase, a quartz crystal phase, and a spinel phase.

[0013] Optionally, the fracture toughness of the glass-ceramics is greater than 1.4 MPa / m 2 The three-point bending strength is not less than 680MPa, and the hot bending temperature is 600-800℃.

[0014] A second aspect of the present disclosure provides a wearable device, wherein the wearable device includes the aforementioned microcrystalline glass.

[0015] The third aspect of the present disclosure provides a method for preparing the aforementioned microcrystalline glass, the method comprising: weighing each raw material and subjecting it to ball milling treatment to obtain raw material powder; subjecting the raw material powder to melting treatment to obtain glass liquid; placing the glass liquid in a mold for annealing treatment to obtain a first material; subjecting the first material to nucleation treatment and crystallization treatment in sequence to obtain a second material; placing the second material in a salt solution for salt bath treatment to obtain microcrystalline glass; wherein the raw material components include substrate components, the substrate components include SiO2, Al2O3, B2O3, SrO, SnO2, ZnO, Bi2O3 and Li2O, as well as at least one component of MgO and CaO, and at least one component of TiO2 and ZrO2.

[0016] Optionally, the substrate component further contains Na2O.

[0017] Optionally, the raw material components further include a color-developing component; the color-developing component is selected from at least one of CuO, Fe2O3, NiO2, MnO2 and CoO2; the salt solution includes strengthening ions, and the strengthening ions are selected from Na + and K + At least one of;

[0018] Optionally, the salt solution contains color-developing ions, and the color-developing ions are selected from Cu 2+ , Fe 3+ 、Ni 4+ , Mn 4+ and Co 4 + At least one of the following: the depth of the glass surface into which the colored ions are immersed is not less than 20 μm.

[0019] Optionally, the conditions for the melt treatment include: a temperature of 1400-1500°C and a time of 1-2 hours; the conditions for the annealing treatment include: a temperature of 600-700°C and a time of 1-2 hours; the conditions for the nucleation treatment include: a temperature of 750-850°C and a time of 1-2 hours; the conditions for the crystallization treatment include: a temperature of 800-1000°C and a time of 1-5 hours; the conditions for the salt bath treatment include: a temperature of 300-600°C and a time of 2-12 hours.

[0020] A fourth aspect of the present disclosure provides a wearable device, comprising the microcrystalline glass prepared by the aforementioned method.

[0021] Through the above technical solution, the microcrystalline glass disclosed in the present invention has the properties of scratch resistance, drop resistance, and easy processing. When applied to a shell, it can achieve a transparent effect and enrich the aesthetic effect of the shell.

[0022] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. DETAILED DESCRIPTION

[0024] A first aspect of the present disclosure provides a glass-ceramic, which contains, based on the total weight of the glass-ceramic, 40 to 60 weight percent SiO2, 2 to 18 weight percent Al2O3, 6 to 22 weight percent B2O3, 2 to 8 weight percent SrO, 2 to 8 weight percent SnO2, 5 to 15 weight percent ZnO, 0.1 to 10 weight percent Bi2O3, 0 to 12 weight percent MgO, 0 to 12 weight percent CaO, 0.1 to 10 weight percent Li2O, 0 to 18 weight percent TiO2 and 0 to 20 weight percent ZrO2; wherein the glass-ceramic includes at least one component of MgO and CaO, and at least one component of TiO2 and ZrO2.

[0025] The microcrystalline glass disclosed in the present invention contains one of spodumene crystal phase, quartz crystal phase and spinel phase, has the properties of scratch resistance, drop resistance and easy processing, and when applied to a shell, can achieve a transparent effect and enrich the aesthetic effect of the shell.

[0026] In the microcrystalline glass disclosed in the present invention, SiO2 and B2O3 are glass network formers and are key components for forming glass; appropriate amounts of Al2O3 and Bi2O3 can serve as glass network intermediates to increase the stability of the glass, and appropriate amounts of SrO and SnO2 can serve as glass clarifiers to promote the removal of bubbles in the glass; appropriate amounts of Li2O can serve as glass network exogens to increase the fluidity of the glass and are essential components for strengthening the glass; appropriate amounts of TiO2 and ZrO2 can serve as nucleating agents to promote the crystallization ability of the glass; ZnO can improve the fluidity and density of the glass, and CaO and MgO can serve as glass solvents to reduce the melting temperature of the glass.

[0027] Exemplarily, based on the total weight of the microcrystalline glass, the microcrystalline glass may contain: 40 to 56 weight % SiO2, 2 to 15 weight % Al2O3, 8 to 20 weight % B2O3, 2 to 8 weight % SrO, 2 to 8 weight % SnO2, 5 to 10 weight % ZnO, 0.1 to 10 weight % Bi2O3, 0 to 12 weight % MgO, 0 to 10 weight % CaO, 0.1 to 10 weight % Li2O, 0 to 15 weight % TiO2 and 0 to 15 weight % ZrO2.

[0028] According to the present disclosure, in the microcrystalline glass, the ratio of the total mass of SiO2 and B2O3 to the total mass of Li2O and Na2O can be 10 to 65, the ratio of the total mass of SrO and SnO2 to the mass of ZnO can be 0.4 to 1.5, the ratio of the total mass of ZnO and Al2O3 to the mass of Li2O can be 4 to 20, and the ratio of the total mass of TiO2 and ZrO2 to the mass of Li2O can be 2 to 30.

[0029] According to the present disclosure, based on the total weight of the microcrystalline glass, the microcrystalline glass may further contain no more than 6 wt% of Na2O. Na2O can serve as a glass network outer body to increase glass fluidity, thereby playing a role in strengthening the glass.

[0030] According to the present disclosure, the microcrystalline glass may further contain coloring ions, and the coloring ions may be selected from Cu 2+ , Fe 3 + 、Ni 4+ , Mn 4+ and Co 4+ At least one of; illustratively, the depth of the glass surface into which the colored ions are immersed is not less than 20 μm.

[0031] According to the present disclosure, the microcrystalline glass may further contain a coloring oxide, and the coloring oxide may be selected from at least one of CuO, Fe2O3, NiO2, MnO2 and CoO2; based on the total weight of the microcrystalline glass, the microcrystalline glass may contain: 0 to 2 weight % of CuO, 0 to 5 weight % of Fe2O3, 0 to 3 weight % of NiO2, 0 to 3 weight % of MnO2, and 0 to 2 weight % of CoO2.

[0032] According to the present disclosure, the crystallization degree of the microcrystalline glass can be 50-95%; the grain size range can be 10-100 nm; when the thickness of the microcrystalline glass is 0.5 mm, the visible light transmittance range can be 20-85%.

[0033] According to the present disclosure, the fracture toughness of the microcrystalline glass can be greater than 1.4 MPa / m 2 The three-point bending strength can be no less than 680MPa, and the hot bending temperature can be 600-800℃.

[0034] A second aspect of the present disclosure provides a wearable device, wherein the wearable device comprises the aforementioned glass-ceramics. Exemplarily, the glass-ceramics in the present disclosure can be used as, but not limited to, a screen cover, a decorative piece, and a structural piece of the wearable device.

[0035] The third aspect of the present disclosure provides a method for preparing the aforementioned microcrystalline glass, the method comprising: weighing raw material components and subjecting them to ball milling treatment to obtain raw material powder; subjecting the raw material powder to melting treatment to obtain glass liquid; placing the glass liquid in a mold for annealing treatment to obtain a first material; subjecting the first material to nucleation treatment and crystallization treatment in sequence to obtain a second material; placing the second material in a salt solution for salt bath treatment to obtain microcrystalline glass; wherein the raw material components include substrate components, the substrate components include SiO2, Al2O3, B2O3, SrO, SnO2, ZnO, Bi2O3 and Li2O, as well as at least one component of MgO and CaO, and at least one component of TiO2 and ZrO2.

[0036] According to the present disclosure, the substrate component may further contain Na2O.

[0037] According to the present disclosure, the raw material components may further include a color-developing component; the color-developing component may be selected from at least one of CuO, Fe2O3, NiO2, MnO2 and CoO2; the salt solution may include strengthening ions, the strengthening ions being selected from Na + and K + At least one of .

[0038] According to the present disclosure, the salt solution may contain color-developing ions, and the color-developing ions may be selected from Cu 2+ , Fe 3+ 、Ni 4+ , Mn 4+ and Co 4+ At least one of .

[0039] In an exemplary embodiment of the present disclosure, the method for preparing colored microcrystalline glass may be: when mixing raw materials, only the necessary components of glass are mixed, and after the glass is formed, it is colored by a salt bath to form the final glass. 2+ , Fe 3+ 、Ni 4+ , Mn 4+ and Co 4+ At least one of the following. After the salt bath, the corresponding coloring ions will be introduced at a certain depth on the glass surface to color the glass surface, increasing the surface stress to achieve a certain strengthening effect, so the glass after the salt bath coloring does not need additional strengthening. The salt bath ion exchange depth under this condition can range from 20 to 70 um.

[0040] In an exemplary embodiment of the present disclosure, a method for preparing colored microcrystalline glass may be: in the process of mixing raw materials, all raw materials (including necessary raw material components and color-developing components) are mixed, and then ball milling, melting, etc. are performed to form glass and then strengthened. For example, the salt solution may contain Na+ and K + At least one of the following: the color-developing component is selected from at least one of CuO, Fe2O3, NiO2, MnO2 and CoO2.

[0041] According to the present disclosure, the conditions of the melting treatment may include: a temperature of 1400-1500°C and a time of 1-2 hours; the conditions of the annealing treatment may include: a temperature of 600-700°C and a time of 1-2 hours; the conditions of the nucleation treatment may include: a temperature of 750-850°C and a time of 1-2 hours; the conditions of the nucleation treatment may include: a temperature of 800-1000°C and a time of 1-5 hours; the conditions of the salt bath treatment may include: a temperature of 300-600°C and a time of 2-12 hours. Wherein, when a salt solution containing coloring ions is used for salt bath treatment, the conditions of the salt bath treatment determine the depth of the coloring ions immersing into the surface of the microcrystalline glass. Exemplarily, the salt bath temperature is 300-450°C, the salt bath time is 2-3h, and the ion immersion depth is not less than 20μm; the salt bath temperature is 300-450°C, the salt bath time is 3-4h, and the ion immersion depth is not less than 30μm; the salt bath temperature is 300-450°C, the salt bath time is 4-5h, and the ion exchange depth is not less than 40μm; the salt bath temperature is 450-600°C, the salt bath time is 5-7h, and the ion exchange depth is not less than 50μm; the salt bath temperature is 450-600°C, the salt bath time is 7-9h, and the ion exchange depth is not less than 60μm; the salt bath temperature is 450-600°C, the salt bath time is 9-12h, and the ion exchange depth is not less than 70μm.

[0042] A fourth aspect of the present disclosure provides a wearable device, wherein the wearable device comprises the glass-ceramic prepared by the above method. Exemplarily, the glass-ceramic in the present disclosure can be used as, but not limited to, a screen cover, a decorative part, and a structural part of the wearable device.

[0043] The present disclosure is further described in detail below through examples. The raw materials used in the examples can be obtained through commercial channels. The test method for the flexural strength in the examples is the three-point bending method; the calculation method for the fracture toughness is: Among them, K IC is the fracture toughness, unit is MPa*m 1 / 2 ; P is the loading force, unit is N; C is the half crack length, unit is m; H is the hardness of the object being tested; E is the elastic modulus.

[0044] Examples 1-5

[0045] Weigh raw material components and perform ball milling to obtain raw material powder; melt the raw material powder to obtain glass liquid; place the glass liquid in a mold for annealing to obtain a first material; perform nucleation treatment and crystallization treatment on the first material in sequence to obtain a second material; place the second material in a salt solution for salt bath treatment to obtain microcrystalline glass; wherein the raw material components are composed of SiO2, Al2O3, B2O3, SrO, SnO2, ZnO, Bi2O3, Li2O, Na2O, and at least one component of MgO and CaO, and at least one component of TiO2 and ZrO2; the salt solution contains Na + and K + The contents of some components of Examples 1-5 and the parameters of the prepared glass-ceramics are shown in Table 1.

[0046] Table 1

[0047]

[0048] Embodiment 6-10

[0049] Weigh raw material components and perform ball milling to obtain raw material powder; melt the raw material powder to obtain glass liquid; place the glass liquid in a mold for annealing to obtain a first material; perform nucleation treatment and crystallization treatment on the first material in sequence to obtain a second material; place the second material in a salt solution for salt bath treatment to obtain microcrystalline glass; wherein the raw material components include a substrate component and a coloring component, the substrate component is composed of SiO2, Al2O3, B2O3, SrO, SnO2, ZnO, Bi2O, Li2O, Na2O, and at least one component of MgO and CaO, at least one component of TiO2 and ZrO2, and the coloring component is selected from at least one of CuO, Fe2O3, NiO2, MnO2 and CoO2, wherein 0 to 2 weight % of CuO, 0 to 5 weight % of Fe2O3, 0 to 3 weight % of NiO2, 0 to 3 weight % of MnO2, and 0 to 2 weight % of CoO2; the salt solution contains Na + and K + The contents of some components of Examples 6-10 and the parameters of the prepared glass-ceramics are shown in Table 2.

[0050] Table 2

[0051]

[0052]

[0053] Examples 11-15

[0054] Weigh raw material components and perform ball milling to obtain raw material powder; melt the raw material powder to obtain glass liquid; place the glass liquid in a mold for annealing to obtain a first material; perform nucleation and crystallization treatments on the first material in sequence to obtain a second material; place the second material in a salt solution for salt bath treatment to obtain microcrystalline glass; wherein the raw material components are composed of SiO2, Al2O3, B2O3, SrO, SnO2, ZnO, Bi2O3, Li2O, Na2O, and at least one component of MgO and CaO, and at least one component of TiO2 and ZrO2; the salt solution contains Cu 2+ , Fe 3+ 、Ni 4+ , Mn 4+ and Co 4+ At least one of .

[0055] The specific components, step parameters and parameters of the prepared microcrystalline glass of Examples 11-15 are shown in Table 3.

[0056] Table 3

[0057]

[0058]

[0059] It can be seen from Examples 1-15 that the fracture toughness of the glass-ceramics prepared in the present invention is greater than 1.4 MPa / m 2 The three-point bending strength is not less than 680MPa, and it has good processing resistance.

[0060] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the present disclosure. This application is intended to cover any variations, uses or adaptations of the present disclosure, which follow the general principles of the present disclosure and include common knowledge or customary technical means in the art that are not disclosed in the present disclosure. The specification and examples are to be considered as exemplary only, and the true scope and spirit of the present disclosure are indicated by the following claims.

[0061] It should be understood that the present disclosure is not limited to the exact construction that has been described and illustrated above and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. A glass-ceramic, characterized in that: Based on the total weight of the microcrystalline glass, the microcrystalline glass contains: 40-60 weight % of SiO2, 2-18 weight % of Al2O3, 6-22 weight % of B2O3, 2-8 weight % of SrO, 2-8 weight % of SnO2, 5-15 weight % of ZnO, 0.1-10 weight % of Bi2O3, 0-12 weight % of MgO, 0-12 weight % of CaO, 0.1-10 weight % of Li2O, 0-18 weight % of TiO2 and 0-20 weight % of ZrO2; Wherein, the microcrystalline glass includes at least one component of MgO and CaO, and at least one component of TiO2 and ZrO2.

2. The glass-ceramic according to claim 1, characterized in that: Based on the total weight of the microcrystalline glass, the microcrystalline glass contains: 40 to 56 weight % SiO2, 2 to 15 weight % Al2O3, 8 to 20 weight % B2O3, 2 to 8 weight % SrO, 2 to 8 weight % SnO2, 5 to 10 weight % ZnO, 0.1 to 10 weight % Bi2O3, 0 to 12 weight % MgO, 0 to 10 weight % CaO, 0.1 to 10 weight % Li2O, 0 to 15 weight % TiO2 and 0 to 15 weight % ZrO2.

3. The glass-ceramic according to claim 1, characterized in that: In the glass-ceramics, The ratio of the total mass of SiO2 and B2O3 to the total mass of Li2O and Na2O is 10 to 65. The ratio of the total mass of SrO and SnO2 to the mass of ZnO is 0.4 to 1.

5. The ratio of the total mass of ZnO and Al2O3 to the mass of Li2O is 4 to 30. The ratio of the total mass of TiO2 and ZrO2 to the mass of Li2O is 2-27.

4. The glass-ceramic according to claim 1, characterized in that: Based on the total weight of the microcrystalline glass, the microcrystalline glass also contains no more than 6 weight % of Na2O.

5. The glass-ceramic according to claim 1, characterized in that: The microcrystalline glass also contains coloring ions, and the coloring ions are selected from Cu 2+ , Fe 3+ 、Ni 4+ , Mn 4+ and Co 4+ At least one of the following: the depth of the glass surface into which the colored ions are immersed is not less than 20 μm.

6. The glass-ceramic according to claim 1, characterized in that: The microcrystalline glass also contains a coloring oxide, which is selected from at least one of CuO, Fe2O3, NiO2, MnO2 and CoO2; based on the total weight of the microcrystalline glass, the microcrystalline glass contains: 0 to 2 weight % CuO, 0 to 5 weight % Fe2O3, 0 to 3 weight % NiO2, 0 to 3 weight % MnO2, and 0 to 2 weight % CoO2.

7. The glass-ceramics according to any one of claims 1 to 6, characterized in that: The crystallization degree of the microcrystalline glass is 50-95%; the grain size range is 10-100nm; when the thickness of the microcrystalline glass is 0.5mm, the visible light transmittance range is 20-85%.

8. The glass-ceramics according to any one of claims 1 to 6, characterized in that: The microcrystalline glass includes at least one of a spodumene crystal phase, a quartz crystal phase, and a spinel phase.

9. The glass-ceramics according to any one of claims 1 to 6, characterized in that: The fracture toughness of the glass-ceramics is greater than 1.4 MPa / m 2 The three-point bending strength is not less than 680MPa, and the hot bending temperature is 600-800℃.

10. A wearable device, characterized in that: The wearable device comprises the glass-ceramic according to any one of claims 1 to 9.

11. A method for preparing the glass-ceramics according to any one of claims 1 to 9, characterized in that: The method comprises: Weighing raw material components and subjecting them to ball milling to obtain raw material powder; Melting the raw material powder to obtain glass liquid; placing the glass liquid in a mold for annealing to obtain a first material; The first material is subjected to a nucleation treatment and a crystallization treatment in sequence to obtain a second material; placing the second material in a salt solution for salt bath treatment to obtain microcrystalline glass; The raw material components include substrate components, and the substrate components include SiO2, Al2O3, B2O3, SrO, SnO2, ZnO, Bi2O3 and Li2O, as well as at least one component of MgO and CaO, and at least one component of TiO2 and ZrO2.

12. The method according to claim 11, characterized in that The substrate component also contains Na2O.

13. The method according to claim 11 or 12, characterized in that: The raw material components also include color-developing components; the color-developing components are selected from at least one of CuO, Fe2O3, NiO2, MnO2 and CoO2; the salt solution includes strengthening ions, and the strengthening ions are selected from Na + and K + At least one of .

14. The method according to claim 11 or 12, characterized in that: The salt solution contains color-developing ions, which are selected from Cu 2+ , Fe 3+ 、Ni 4+ , Mn 4+ and Co 4+ At least one of .

15. The method according to claim 11, characterized in that The conditions of the melt treatment include: a temperature of 1400-1500°C and a time of 1-2h; The annealing conditions include: a temperature of 600 to 700° C. and a time of 1 to 2 hours; The conditions of the nucleation treatment include: a temperature of 750 to 850°C and a time of 1 to 2 hours; The crystallization treatment conditions include: a temperature of 800 to 1000° C. and a time of 1 to 5 hours; The conditions of the salt bath treatment include: a temperature of 300 to 600° C. and a time of 2 to 12 hours.

16. A wearable device, characterized in that: The wearable device comprises glass-ceramics prepared by the method described in any one of claims 11-15.

Citation Information

Patent Citations

  • Optical glass

    CN101712530A

  • Photocatalyst, slurry mixture, forming member and coating, coating film forming member, sintered body, glass-ceramic composite, glass, building material and clarification material

    CN102947001A

  • Glass ceramics and substrate thereof

    CN107915412A

  • Glass ceramic product, glass ceramic and manufacturing method thereof

    CN110510879A

  • Glass and magnetic head

    JP1992031337A