A kind of high wear-resistant concrete and preparation method thereof

By depositing tungsten carbide nanoparticles loaded with calcium silicate in cement concrete and forming porous structures, combined with the treatment of coal gangue and apatite, the problems of damage and wear resistance of cement concrete pavement under traffic loads are solved, and the problem of loss of wear resistance of cement concrete pavement is achieved. Higher wear resistance and impact strength.

CN118724541BActive Publication Date: 2024-11-19DEZHOU RUNDE CONCRETE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411227254.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-19
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Cement concrete pavement is prone to damage and tear under traffic loads, and tungsten carbide nanoparticles are brittle and easy to corrode, resulting in a degradation of wear resistance.

Method used

By depositing calcium silicate-loaded tungsten carbide nanoparticles on the surface of mullite fibers, mixing them with silica sol and glucose at high temperature to form a porous structure, increasing the distribution of silicon carbide nanowires; at the same time, coal gangue and phosphate two Ammonium hydrogen and calcium nitrate tetrahydrate are mixed to form hydroxyapatite nanoparticles, and fulvic acid reacts with lactic acid monomer to increase the degree of branching of polylactic acid.

Benefits of technology

It improves the impact resistance and corrosion resistance of tungsten carbide, enhances the wear resistance and impact strength of concrete, extends the service life, reduces the rise in road surface temperature and reduces thermal damage.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high wear-resistant concrete and a preparation method thereof, which belongs to the technical field of wear-resistant concrete, and comprises the following steps: depositing tungsten carbide nanoparticles loaded with calcium silicate on the surface of mullite fiber, mixing with silica sol and glucose, and pyrolyzing at high temperature to obtain a wear-resistant agent; reacting fulvic acid with lactic acid monomer, and then adding coal gangue and polyethylene glycol loaded with hydroxyapatite to obtain a composite material; mixing cement, river sand, crushed stone, fly ash, mineral powder, wear-resistant agent, and composite material, and then adding a water reducer and water, stirring to obtain a high wear-resistant concrete. Anisotropic silicon carbide nanowires are evenly distributed in the space between mullite fibers and interweave to form a porous structure, which reduces the temperature rise of concrete under direct sunlight and reduces thermal damage to the road surface; hydroxyapatite is formed on the surface of coal gangue to complete the fixation of heavy metals in coal gangue, and the heavy metals in coal gangue are prevented from being released into concrete, resulting in a decrease in the wear resistance of concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wear-resistant concrete, in particular to high-wear-resistant concrete and a preparation method thereof. Background Art

[0002] Cement concrete pavement is a rigid pavement. Compared with ordinary asphalt concrete pavement, it has the advantages of high bearing capacity, good stability, long service life, long flatness retention period, less environmental pollution and low maintenance cost. Therefore, cement concrete pavement is widely used in highways, urban roads, squares, parking lots, airport runways, stations and docks, etc. Cement concrete pavement not only requires high strength, low brittleness and good impact toughness, but also should have excellent wear resistance. The wear resistance of cement concrete pavement is mainly improved by adding mineral admixtures, reinforcing materials and improving the construction technology of road projects, and the wear resistance is improved through stress transfer and crack bridging, so as to achieve excellent road performance of cement concrete pavement.

[0003] Cement concrete pavement not only requires high strength, low brittleness, and good impact toughness, but also excellent wear resistance. Cement concrete aggregate particles are worn or crushed by the tires of moving vehicles, causing excessive damage and tearing of the concrete under traffic loads. Adding tungsten carbide particles to concrete aggregate can effectively improve the wear resistance of concrete, but tungsten carbide nanoparticles are brittle and become brittle under external forces, resulting in a decrease in wear resistance. In addition, as the humidity of the concrete increases, the tungsten carbide particles are easily corroded. Summary of the invention

[0004] The purpose of the present invention is to provide a high wear-resistant concrete and a preparation method thereof: wear-resistant aggregate is mixed with silicate, treated with hydrochloric acid, so that calcium silicate is coated on the surface of tungsten carbide, the impact resistance and corrosion resistance of tungsten carbide are improved, and the corrosion of nano tungsten carbide due to increased humidity in concrete is avoided, resulting in a decrease in wear resistance; tungsten carbide nanoparticles loaded with calcium silicate are deposited on the surface of mullite fibers, silica sol and glucose are added, and pyrolysis is performed at high temperature, so that anisotropic silicon carbide nanowires are evenly distributed in the space between mullite fibers and interweave to form a porous structure, thereby reducing heat conduction and reducing the temperature rise of road surface concrete under direct sunlight, thereby reducing thermal damage to the road surface, and the silicon hydroxyl group contained in the calcium silicate in the nanoparticles can The wear-resistant agent can be combined with aggregate particles through chemical bonds, and the wear-resistant agent is evenly dispersed in the concrete matrix, increasing the bonding force between the wear-resistant agent and the concrete; the coal gangue is mixed with ammonium dihydrogen phosphate and calcium nitrate tetrahydrate, and then subjected to hydrothermal treatment to form hydroxyapatite nanoparticles on the surface of the coal gangue. The hydroxyl and phosphate groups contained in the nanoparticles can combine with the metal ions in the coal gangue to fix the heavy metals in the coal gangue; fulvic acid reacts with lactic acid monomers to graft fulvic acid on polylactic acid, significantly increasing the branching degree and intermolecular distance of polylactic acid, and increasing the mutual sliding between molecular chains. When the concrete is impacted, the energy is dispersed through the movement of the chain segments and absorbed by the movement of the chain segments, and has excellent impact strength.

[0005] The technical problem to be solved by the present invention is as follows: Cement concrete pavement not only requires high strength, low brittleness, and good impact toughness, but also should have excellent wear resistance. Cement concrete aggregate particles are worn or crushed by the tires of traveling vehicles, resulting in excessive damage and tearing of the concrete under traffic loads. Adding tungsten carbide particles to concrete aggregate can effectively improve the wear resistance of concrete, but tungsten carbide nanoparticles are brittle and become brittle under the action of external forces, resulting in decreased wear resistance. In addition, as the humidity of the concrete increases, the tungsten carbide particles are easily corroded.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing highly wear-resistant concrete comprises the following steps:

[0008] S1. The tungsten carbide nanoparticles loaded with calcium silicate are deposited on the surface of the mullite fiber, and then mixed with silica sol and glucose, and pyrolyzed at high temperature to obtain a wear-resistant agent;

[0009] Furthermore, the diameter of the mullite fiber is 200-300 nm and the length is 0.1-2 μm.

[0010] More preferably, the diameter of the mullite fiber is 200-250 nm and the length is 0.1-1 μm.

[0011] More preferably, the diameter of the mullite fiber is 230 nm and the length is 0.5 μm.

[0012] Furthermore, the silica sol is prepared by mixing organic silicon, deionized water and sodium hydroxide in a mass ratio of (0.5-1.5):(50-60):(5-8).

[0013] Furthermore, the organosilicon is selected from one of tetraethyl silicate, tetrakis(2-methoxyethoxy)silane, tetrakis(trimethylsiloxy)silane, and methyltris(trimethylsiloxy)silane.

[0014] More preferably, the organosilicon is selected from tetraethyl silicate and tetrakis(2-methoxyethoxy)silane.

[0015] More preferably, the organosilicon is selected from tetraethyl silicate.

[0016] Furthermore, the high temperature pyrolysis temperature is 1200-1400°C and the time is 2-5h.

[0017] More preferably, the high temperature pyrolysis temperature is 1300° C. and the time is 3 h.

[0018] Further, the anti-wear agent is prepared by the following steps:

[0019] A1. Add tungsten carbide nanoparticles loaded with calcium silicate into ethanol, stir evenly, add ethylene glycol and hydrochloric acid with a mass dispersion of 36%, stir to obtain a dispersion, immerse mullite fiber into the dispersion so that the nanoparticles are evenly coated on the fiber surface, stir at 80°C until the organic solvent evaporates, place in a 70°C oven and dry for 10 minutes to obtain modified mullite fiber.

[0020] Among them, the oxygen-containing functional groups contained on the surface of tungsten carbide nanoparticles loaded with calcium silicate and mullite fibers can be combined with the hydroxyl groups of ethylene glycol through chemical bonds, so that the tungsten carbide nanoparticles loaded with calcium silicate are deposited on the surface of the mullite fibers, blocking the pores on the surface of the mullite fibers and reducing the hygroscopicity of the fibers. The mullite fibers can be filled into the pores of the concrete, thereby increasing the density and enhancing the wear resistance.

[0021] Furthermore, the dosage ratio of tungsten carbide nanoparticles loaded with calcium silicate, ethanol, ethylene glycol, and hydrochloric acid is (0.3-0.7) g: (25-35) mL: (0.03-0.07) g: (1-3) mL.

[0022] A2. Mix organosilicon, deionized water and sodium hydroxide, stir evenly to form silica sol, add nitric acid with a mass fraction of 68% to the silica sol to adjust the pH to 3.5 to promote the hydrolysis of organosilicon, and obtain a mixed solution, add glucose to deionized water, stir in a 40°C water bath for 30 minutes, add the mixed solution, stir for 30 minutes, add modified mullite fiber, stir at 50°C for 2 hours, place in a closed reactor, introduce argon, pyrolyze at 1300°C for 3 hours, cool to room temperature, and obtain a wear-resistant agent;

[0023] Among them, mullite fiber is used as a template, silica sol is used as a silicon source, and glucose is used as a carbon source. After high-temperature pyrolysis, the silicon source is pyrolyzed to form silicon monoxide gas, which can react with the carbon element on the surface of the mullite fiber to form silicon carbide crystal nuclei, providing growth sites for the growth of silicon carbide nanowires.

[0024] Further, the pyrolysis is continued, and the pyrolysis of glucose provides a large amount of carbon monoxide gas, which continues to react with silicon monoxide to form silicon carbide nanowires on the surface of the mullite fiber. The formed silicon carbide nanowires can fill the micropores inside the concrete, reduce the permeability and porosity of the concrete, and thus improve its impermeability and freeze-thaw resistance.

[0025] Furthermore, anisotropic silicon carbide nanowires are evenly distributed in the space between mullite fibers and interweave to form a porous structure, which effectively reduces heat conduction, reduces the temperature rise of pavement concrete under direct sunlight, and reduces thermal damage to the road surface; the nanoparticles loaded on the fiber surface can be filled into the interweaving porous structure, refine the pore size, increase the porosity, and enhance the thermal insulation performance.

[0026] Furthermore, the dosage ratio of silica sol, glucose, deionized water and modified mullite fiber is (8-12) mL: (3-4) g: (35-45) mL: (0.6-0.7) g.

[0027] Furthermore, the calcium silicate-loaded tungsten carbide nanoparticles are prepared by mixing wear-resistant aggregate and silicate and treating with hydrochloric acid.

[0028] Furthermore, the wear-resistant aggregate is selected from one of nano-tungsten carbide, nano-silicon dioxide, nano-titanium dioxide, nano-zirconium dioxide, nano-calcium oxide, and nano-calcium carbonate.

[0029] Further preferably, the wear-resistant aggregate is selected from one of nano-tungsten carbide, nano-silicon dioxide, nano-titanium dioxide and nano-zirconium dioxide.

[0030] Further preferably, the wear-resistant aggregate is selected from nano-tungsten carbide.

[0031] Furthermore, the silicate is selected from one of calcium silicate, sodium silicate and aluminum silicate.

[0032] More preferably, the silicate is selected from calcium silicate and sodium silicate.

[0033] Further preferably, the silicate is selected from calcium silicate.

[0034] Further, the calcium silicate-loaded tungsten carbide nanoparticles are prepared by the following steps:

[0035] The silicate particles were placed in 0.1 mol / L hydrochloric acid and stirred at 300 prm for 10 min to form a composite slurry. Wear-resistant aggregate nano-tungsten carbide was added to the composite slurry and stirred for 30 min. The slurry was filtered, washed with deionized water for 3 times, and dried in an oven at 70°C for 10 min to obtain tungsten carbide nanoparticles loaded with calcium silicate.

[0036] Among them, after calcium silicate is acidified with hydrochloric acid, a stable silicon dioxide layer is formed on the surface of calcium silicate particles. The silanol groups on the surface of calcium silicate particles can be combined with the hydroxyl groups on the surface of tungsten carbide particles through chemical bonds, so that calcium silicate is coated on the surface of tungsten carbide, thereby improving the impact resistance of tungsten carbide. The silicon dioxide layer contained in it has excellent corrosion resistance, thereby improving the corrosion resistance of tungsten carbide and preventing nano tungsten carbide from being easily corroded due to increased humidity in concrete, resulting in a decrease in wear resistance.

[0037] Furthermore, the amount ratio of silicate particles, hydrochloric acid and wear-resistant aggregate is (2-3) g: (8-12) mL: (0.3-0.7) g.

[0038] S2. reacting fulvic acid with lactic acid monomer, and then adding coal gangue loaded with hydroxyapatite and polyethylene glycol to obtain a composite material, which is specifically prepared by the following steps:

[0039] B1. Add fulvic acid and lactic acid monomers to a round-bottom flask, heat to 115°C until completely dissolved, add stannous octoate, stir for 30 minutes, evacuate to 0.095 MPa, continue to react for 2 hours, cool to room temperature, add chloroform to dissolve the product, centrifuge at 8000 rpm for 10 minutes to remove the supernatant, collect the precipitate, wash the precipitate with deionized water 3 times, and dry in an oven at 40°C for 2 hours to obtain fulvic acid-grafted polylactic acid;

[0040] Among them, under the action of the catalyst stannous octoate, the hydroxyl group in the lactic acid monomer can undergo esterification reaction with the carboxyl group in the fulvic acid, and the lactic acid monomer is polymerized to form polylactic acid, thereby realizing the grafting of fulvic acid onto the polylactic acid. The degree of branching and the intermolecular distance of the polylactic acid are significantly increased, and the mutual sliding between the molecular chains is increased. When the concrete is impacted, the energy is dispersed through the movement of the chain segments and absorbed by the movement of the chain segments, and has excellent impact strength.

[0041] Furthermore, the mass ratio of fulvic acid, lactic acid monomer, and stannous octoate is (1-2) g:(8.5-9.4) g:(0.3-0.7) g.

[0042] B2. The fulvic acid-grafted polylactic acid, hydroxyapatite-loaded coal gangue and polyethylene glycol were added to deionized water, stirred until uniform, and dried in an oven at 80°C to obtain a composite material.

[0043] Among them, the oxygen-containing functional groups in the fulvic acid-grafted polylactic acid are combined with the hydroxyl groups of polyethylene glycol through chemical bonds to form a three-dimensional cross-linked network gel, and the hydroxyl groups on the surface of the stone coal gangue loaded with hydroxyapatite can react with the oxygen-containing functional groups in the three-dimensional cross-linked network gel, thereby increasing the cross-linking density of the gel composite, having higher toughness, being dispersed in the concrete, and improving the mechanical strength of the concrete.

[0044] Furthermore, the mass ratio of fulvic acid grafted polylactic acid, hydroxyapatite loaded coal gangue, and polyethylene glycol is (10-11) g:(1-2) g:(4-5) g.

[0045] Furthermore, the hydroxyapatite-loaded coal gangue is prepared by mixing coal gangue with ammonium dihydrogen phosphate and calcium nitrate tetrahydrate, and then subjecting the mixture to hydrothermal treatment;

[0046] Furthermore, the silica content in the coal gangue is 28-30%; the alumina content is 26-28%; and the iron oxide content is 3.8-4.8%.

[0047] More preferably, the silicon dioxide content in the coal gangue is 28-29%; the aluminum oxide content is 26-27%; and the iron oxide content is 3.8-4.5%.

[0048] Further preferably, the silicon dioxide content in the coal gangue is 28.9%; the aluminum oxide content is 26.5%; and the iron oxide content is 4.1%.

[0049] Furthermore, the hydrothermal treatment temperature is 100-200°C, and the hydrothermal reaction time is 2-6h.

[0050] More preferably, the hydrothermal treatment temperature is 100-150° C., and the hydrothermal reaction time is 2-5 h.

[0051] More preferably, the hydrothermal treatment temperature is 120° C. and the hydrothermal reaction time is 3 h.

[0052] Further, the hydroxyapatite-loaded coal gangue is prepared by the following steps:

[0053] The gangue was washed with deionized water, naturally aired to dry, and ground into powder to obtain gangue powder. The gangue powder was added to a sodium dodecyl sulfate solution, stirred evenly, and 3.2 mol / L of ammonium dihydrogen phosphate and calcium nitrate tetrahydrate were added. The mixture was stirred at a rate of 500 r / min for 2 h, stirred at 120°C for 3 h, filtered, washed with deionized water 3 times, and dried in an oven at 70°C for 10 min to obtain hydroxyapatite-loaded stone gangue.

[0054] Among them, in the sodium dodecyl sulfate solution, the hydroxyl groups carried on the surface of the coal gangue can combine with the calcium ions in the calcium nitrate tetrahydrate, so that the calcium particles are adsorbed on the surface of the coal gangue, and the calcium ions continue to combine with the phosphate ions in the diammonium phosphate to form a calcium phosphate complex. After hydrothermal treatment, the calcium phosphate complex is crystallized to form 20-30nm hydroxyapatite nanoparticles on the surface of the coal gangue. The hydroxyl and phosphate groups contained on the surface can combine with the metal ions in the coal gangue to fix the heavy metals in the coal gangue, thereby preventing the heavy metals in the coal gangue from being released into the concrete and causing the performance of the concrete to deteriorate.

[0055] Furthermore, the usage ratio of coal gangue powder, sodium dodecyl sulfate solution, ammonium dihydrogen phosphate, and calcium nitrate tetrahydrate is (1-2) g: (15-25) mL: (18-22) mL: (6-7) g.

[0056] S3. Mix cement, river sand, crushed stone, fly ash, mineral powder, wear-resistant agent and composite material, then add water reducing agent and water, stir and obtain high wear-resistant concrete.

[0057] Furthermore, the cement is silicate cement with a PO4 of 2.5 and a 28d compressive strength of 56.3 MPa.

[0058] Furthermore, the river sand is Grade II medium sand, with a fineness modulus of 2.9 and a mud content of 1.6%.

[0059] Furthermore, the crushed stone particle size is 5-10 mm and the mud content is 0.4%.

[0060] Furthermore, the fly ash is Class II fly ash with a specific surface area of ​​225m 2 / kg, the fineness of fly ash is 23-46μm.

[0061] Furthermore, the mineral powder is S95 grade mineral powder with a specific surface area of ​​450m 2 / kg, and the activity index at 28 days was 95%.

[0062] Furthermore, the water reducer is any one of PCE-102 polycarboxylate water reducer, PCE-101 polycarboxylate water reducer, and PCE-103 polycarboxylate water reducer.

[0063] Furthermore, compared with the prior art, the present invention has the following beneficial effects:

[0064] (1) In the technical scheme of the present invention, after the calcium silicate particles are acidified, a stable silicon dioxide layer is formed on the surface of the calcium silicate particles. The silanol groups on the surface of the calcium silicate particles can be combined with the hydroxyl groups on the surface of the tungsten carbide particles through chemical bonds, so that the calcium silicate is coated on the surface of the tungsten carbide, thereby improving the impact resistance of the tungsten carbide. The silicon dioxide layer contained in the calcium silicate particles has excellent corrosion resistance, thereby improving the corrosion resistance of the tungsten carbide and preventing the nano-tungsten carbide from being easily corroded due to the increase in humidity in the concrete, thereby causing the wear resistance to decrease. The tungsten carbide nanoparticles loaded with calcium silicate are deposited on the surface of the mullite fiber, blocking the pores on the surface of the mullite fiber and reducing the hygroscopicity of the fiber. The mullite fiber can be filled into the pores of the concrete, thereby improving the density and enhancing the wear resistance.

[0065] (2) In the technical solution of the present invention, mullite fiber is used as a template, silica sol is used as a silicon source, and glucose is used as a carbon source. After high-temperature pyrolysis, silicon carbide nanowires are formed on the surface of the mullite fiber. The anisotropic silicon carbide nanowires are evenly distributed in the space between the mullite fibers and interweave to form a porous structure. The structure has excellent thermal insulation performance, effectively reduces heat conduction, and reduces the temperature rise of road concrete under direct sunlight, thereby reducing thermal damage to the road surface. In addition, the thermal expansion coefficient of silicon carbide nanowires is low, which can reduce the expansion strain of concrete caused by temperature changes, thereby improving the thermal insulation performance. High crack resistance. In addition, the nanoparticles loaded on the fiber surface can be filled into the interwoven porous structure, refine the pore size, increase the porosity, and thus enhance the thermal insulation performance. The silanol contained in the calcium silicate in the core-shell nanoparticles can be combined with the aggregate particles through chemical bonds. The wear-resistant agent is evenly dispersed in the concrete matrix, increasing the bonding force between the wear-resistant agent and the concrete. When the concrete is subjected to a large impact load, the wear-resistant agent is not easy to separate from the cementitious material in the concrete, so that the finished concrete has good wear resistance for a long time and extends the service life of the concrete.

[0066] (3) In the technical solution of the present invention, coal gangue has high hardness, high density and high wear resistance. It is added to concrete as a wear-resistant aggregate to improve the wear resistance of concrete. 20-30nm hydroxyapatite nanoparticles are formed on the surface of coal gangue. The hydroxyl and phosphate groups contained on the surface can combine with the metal ions in the coal gangue to fix the heavy metals in the coal gangue, thereby preventing the heavy metals in the coal gangue from being released into the concrete and causing the wear resistance of the concrete to decrease. The formed hydroxyapatite can absorb part of the heat in the cement hydration product process, thereby reducing the possibility of cracks in the recycled concrete due to the temperature difference between the inside and the outside. In addition, the hydroxyl groups contained on the surface of coal gangue and hydroxyapatite as wear-resistant aggregates can be adsorbed on the surface of cement aggregate to increase the wear resistance of concrete.

[0067] (4) In the technical scheme of the present invention, fulvic acid is grafted onto polylactic acid, which significantly increases the branching degree and intermolecular distance of polylactic acid and increases the mutual sliding between molecular chains. When the concrete is impacted, the energy is dispersed and absorbed by the movement of the chain segments, and has excellent impact strength. The fulvic acid-grafted polylactic acid and polyethylene glycol form a three-dimensional cross-linked network gel, and the hydroxyl groups on the surface of the stone coal gangue loaded with hydroxyapatite can react with the oxygen-containing functional groups in the three-dimensional cross-linked network gel, thereby increasing the cross-linking density of the gel composite, having higher toughness, being dispersed in the concrete, and improving the mechanical strength of the concrete. The gel formed by cross-linking polylactic acid and polyethylene glycol has better fluidity and can be better filled into the pores of the concrete, thereby increasing the density. DETAILED DESCRIPTION

[0068] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0069] The reagents used in the embodiments of the present invention are as follows: fulvic acid: (model 479-66-3, purity 89.5%); lactic acid monomer: (model 50-21-5, purity 86.9%, Tianjin Guangfu Technology Development Co., Ltd., China); stannous octoate: (model 301-10-0, purity 95.0%); polyethylene glycol (model 25322-68-3, molecular weight 2000); calcium nitrate tetrahydrate (analytical grade AR, Sinopharm Chemical Reagent Co., Ltd.).

[0070] Embodiment 1, anti-wear agent is prepared by the following steps:

[0071] A1. Place 2.5 g of calcium silicate particles in 10 mL of 0.1 mol / L hydrochloric acid and stir at 300 prm for 10 min to form a composite slurry. Add 0.5 g of nano-tungsten carbide to the composite slurry and continue stirring for 30 min. Filter, wash with deionized water three times, and dry in an oven at 70 ° C for 10 min to obtain tungsten carbide nanoparticles loaded with calcium silicate.

[0072] A2. Add 0.5 g of calcium silicate-loaded tungsten carbide nanoparticles to 30 mL of ethanol, stir evenly, add 0.05 g of ethylene glycol and 2 mL of 36% hydrochloric acid, stir to obtain a dispersion, immerse the mullite fiber in the dispersion, stir at 80 ° C until the organic solvent evaporates, and place in a 70 ° C oven to dry for 10 min to obtain modified mullite fiber;

[0073] A3. Mix 1g of tetraethyl silicate, 55g of deionized water and 6.5g of sodium hydroxide, stir evenly to form silica sol, add 2.5mL of 68% nitric acid to 10mL of silica sol to adjust the pH to 3.5 to obtain a mixed solution, add 3.5g of glucose to 40mL of deionized water, stir in a 40℃ water bath for 30min, add 10mL of the mixed solution, stir for 30min, add 0.65g of modified mullite fiber, stir at 50℃ for 2h, place in a closed reactor, pass argon, pyrolyze at 1300℃ for 3h, cool to room temperature to obtain a wear-resistant agent.

[0074] Comparative Example 1

[0075] The difference between this comparative example and Example 1 is that the tungsten carbide nanoparticles loaded with calcium silicate are replaced with nano-tungsten carbide.

[0076] Comparative Example 2

[0077] The difference between this comparative example and Example 1 is that no tungsten carbide nanoparticles loaded with calcium silicate are added.

[0078] Embodiment 2, composite material is prepared by following steps:

[0079] B1. Wash the gangue with deionized water, dry it naturally in the sun, grind it into powder, and obtain gangue powder. Add 1.5 g of gangue powder to 20 mL of sodium dodecyl sulfate solution, stir evenly, add 20 mL of 3.2 mol / L ammonium dihydrogen phosphate and 6.5 g of calcium nitrate tetrahydrate, stir at 500 r / min for 2 h, stir at 120 ° C for 3 h, filter, wash with deionized water 3 times, and dry in an oven at 70 ° C for 10 min to obtain hydroxyapatite-loaded stone gangue;

[0080] B2. 1.5 g of fulvic acid and 8.9 g of lactic acid monomer were added to a 50 mL round-bottom flask, heated to 115 ° C until completely dissolved, 0.5 g of stannous octoate was added, stirred for 30 min, evacuated to 0.095 MPa, and the reaction was continued for 2 h. The mixture was cooled to room temperature and added to 10 mL of chloroform to dissolve the product. The supernatant was removed by centrifugation at 8000 rpm for 10 min, and the precipitate was collected. The precipitate was washed 3 times with deionized water and dried in an oven at 40 ° C for 2 h to obtain fulvic acid-grafted polylactic acid;

[0081] B3. 10.5 g of fulvic acid-grafted polylactic acid, 1.5 g of hydroxyapatite-loaded coal gangue and 4.5 g of polyethylene glycol-2000 were added to 50 mL of deionized water, stirred until uniform, and dried in an oven at 80 ° C to obtain a composite material.

[0082] Comparative Example 3

[0083] The difference between this comparative example and Example 2 is that the stone coal gangue loaded with hydroxyapatite is replaced by coal gangue.

[0084] Comparative Example 4

[0085] The difference between this comparative example and Example 2 is that the fulvic acid-grafted polylactic acid is replaced by polylactic acid.

[0086] Embodiment 3: A method for preparing highly wear-resistant concrete, comprising the following steps:

[0087] 270g of cement, 630g of river sand, 750g of crushed stone, 60g of fly ash, 48g of mineral powder, 15g of wear-resistant agent and 10g of composite material were mixed, and the above raw materials were mixed and stirred for 3 minutes. 3.5g of PCE-101 polycarboxylate water reducer, 2.5g of PCE-103 polycarboxylate water reducer and 100g of water were added, and stirring was continued for 10 minutes to obtain high wear-resistant concrete.

[0088] Embodiment 4: A method for preparing highly wear-resistant concrete, comprising the following steps:

[0089] 305 g of cement, 675 g of river sand, 800 g of crushed stone, 70 g of fly ash, 58 g of mineral powder, 20 g of wear-resistant agent, and 15 g of reinforcing filler were mixed, and the above raw materials were mixed and stirred for 3 min. 3.5 g of PCE-102 polycarboxylate water-reducing agent, 3 g of PCE-103 polycarboxylate water-reducing agent, and 115 g of water were added, and stirring was continued for 10 min to obtain highly wear-resistant concrete.

[0090] Embodiment 5: A method for preparing highly wear-resistant concrete, comprising the following steps:

[0091] 340g of cement, 725g of river sand, 850g of crushed stone, 80g of fly ash, 68g of mineral powder, 25g of wear-resistant agent, and 20g of reinforcing filler were mixed, and the above raw materials were mixed and stirred for 3 minutes. 3g of PCE-102 polycarboxylate water reducer, 4g of PCE-101 polycarboxylate water reducer and 130g of water were added, and stirring was continued for 10 minutes to obtain high wear-resistant concrete.

[0092] Comparative Example 5

[0093] The difference between this comparative example and Example 4 is that the anti-wear agent is replaced by the substance prepared in Comparative Example 1.

[0094] Comparative Example 6

[0095] The difference between this comparative example and Example 4 is that the anti-wear agent is replaced by the substance prepared in Comparative Example 2.

[0096] Comparative Example 7

[0097] The difference between this comparative example and Example 4 is that the reinforcing filler is replaced by the material prepared in Comparative Example 3.

[0098] Comparative Example 8

[0099] The difference between this comparative example and Example 4 is that the reinforcing filler is replaced by the material prepared in Comparative Example 4.

[0100] The high wear-resistant concrete prepared in Examples 3-5 and Comparative Examples 5-8 was tested for performance; according to the provisions of "Testing Procedures for Cement and Cement Concrete for Highway Engineering" JTGE30-2005 and "Testing Method for Abrasion Resistance of Cement Mortar" JC / T421-1991, a wear test was performed using a TMS-04 cement mortar / concrete wear tester with a flower wheel grinding head, and the wear resistance of the concrete after 28 days was calculated;

[0101] The compressive strength and flexural strength of the prepared concrete were tested according to the testing standard of GB / T50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete". After the prepared concrete was cured for 28 days, it was dried at 110°C for 24 hours, placed in a high-temperature furnace, and calcined at a constant temperature of 400°C for 3 hours, and then naturally cooled to room temperature, and the various properties of the concrete after calcination were measured;

[0102] The thermal conductivity of concrete was directly measured using the heat flow meter method. The heat flow and temperature difference of the concrete prepared above were measured using a heat flow method thermal conductivity coefficient tester to calculate the thermal conductivity of the concrete. The test results are shown in Table 1 below:

[0103] .

[0104] It can be seen from the data in Table 1 that in Comparative Example 5, the tungsten carbide nanoparticles loaded with calcium silicate are replaced with nano-tungsten carbide, and the wear resistance of the prepared wear-resistant agent is reduced when it is added to concrete. This may be because calcium silicate is coated on the surface of tungsten carbide, which improves the corrosion resistance of tungsten carbide and enhances the wear resistance of concrete; Comparative Example 6 is tungsten carbide nanoparticles without calcium silicate loading, and the wear resistance and heat resistance of the prepared wear-resistant agent are reduced when it is added to concrete. This may be because the nanoparticles loaded on the fiber surface can be filled into the porous structure, refine the pore size, and enhance the thermal insulation performance, and the silanol contained in the calcium silicate in the core-shell nanoparticles can be combined with the aggregate particles through chemical bonds, thereby increasing the bonding force between the wear-resistant agent and the concrete, and the wear-resistant agent is not easy to separate from the cementitious material in the concrete, has good wear resistance, and prolongs the concrete. Service life; Comparative Example 7 is that the stone coal gangue loaded with hydroxyapatite is replaced by coal gangue, and the prepared composite is added to the concrete, and its thermal insulation performance and compressive strength decrease. This may be because hydroxyapatite nanoparticles are formed on the surface of the coal gangue, and the hydroxyl and phosphate groups contained on the surface can combine with the metal ions in the coal gangue, thereby avoiding the release of heavy metals in the coal gangue into the concrete, resulting in the performance of the concrete being decreased; Comparative Example 8 is that the fulvic acid-grafted polylactic acid is replaced by polylactic acid, and the prepared composite is added to the concrete, and its impact resistance decreases. This may be because the fulvic acid is grafted on the polylactic acid, and the degree of branching and the intermolecular distance of the polylactic acid are significantly increased, which increases the mutual sliding between the molecular chains. When the concrete is impacted, the energy is dispersed through the movement of the chain segments and absorbed by the movement of the chain segments, and has excellent impact strength.

[0105] The data in Table 1 show that the high wear-resistant concrete prepared in Examples 3-5 not only has good wear resistance and impact strength, but also has good bonding between the wear-resistant agent and reinforcing filler and concrete. Tungsten carbide nanoparticles loaded with calcium silicate are deposited on the surface of mullite fiber, mixed with silica sol and glucose, and pyrolyzed at high temperature to obtain a wear-resistant agent; fulvic acid is reacted with lactic acid monomer, and then coal gangue loaded with hydroxyapatite and polyethylene glycol are added to obtain a composite material; cement, river sand, crushed stone, fly ash, mineral powder, wear-resistant agent, composite material are mixed, and then water reducer and water are added and stirred, and the obtained high wear-resistant concrete meets the test performance requirements, while the high wear-resistant concrete prepared in Comparative Examples 5-8 does not meet the performance requirements, indicating that the high wear-resistant concrete prepared by the present invention not only has good wear resistance and impact strength, but also has good bonding between the wear-resistant agent and reinforcing filler and concrete.

[0106] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0107] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing highly wear-resistant concrete, It is characterized in that The following steps are involved: S1. The tungsten carbide nanoparticles loaded with calcium silicate are deposited on the surface of the mullite fiber, and then mixed with silica sol and glucose, and pyrolyzed at high temperature to obtain a wear-resistant agent; The calcium silicate-loaded tungsten carbide nanoparticles are prepared by mixing wear-resistant aggregate and silicate and treating with hydrochloric acid; The wear-resistant aggregate is selected from nano-tungsten carbide; The silicate is selected from one of calcium silicate, sodium silicate and aluminum silicate; S2. The fulvic acid and lactic acid monomers are reacted, and then hydroxyapatite-loaded coal gangue and polyethylene glycol are added to obtain a composite material; The hydroxyapatite-loaded coal gangue is prepared by mixing coal gangue with ammonium dihydrogen phosphate and calcium nitrate tetrahydrate, and then subjecting the mixture to hydrothermal treatment; S3. Mix cement, river sand, crushed stone, fly ash, mineral powder, wear-resistant agent and composite material, then add water reducing agent and water, stir and obtain high wear-resistant concrete.

2. A method for preparing highly wear-resistant concrete according to claim 1, It is characterized in that The mullite fiber has a diameter of 200-300 nm and a length of 0.1-2 μm.

3. A method for preparing a highly wear-resistant concrete according to claim 1, It is characterized in that The silica sol is prepared by mixing organic silicon, deionized water and sodium hydroxide in a mass ratio of (0.5-1.5):(50-60):(5-8).

4. A method for preparing highly wear-resistant concrete according to claim 3, It is characterized in that The organic silicon is selected from tetraethyl silicate, tetrakis(2-methoxyethoxy)silane, tetrakis(trimethylsiloxy)silane, and methyltris(trimethylsiloxy)silane.

5. The method for preparing a highly wear-resistant concrete according to claim 1, It is characterized in that The cement is silicate cement with a PO4 of 2.5 and a 28d compressive strength of 56.3 MPa.

6. The method for preparing a highly wear-resistant concrete according to claim 1, It is characterized in that The fly ash is Grade II fly ash with a specific surface area of ​​225m 2 / kg, the fineness of fly ash is 23-46μm.

7. The method for preparing a highly wear-resistant concrete according to claim 1, It is characterized in that The crushed stone has a particle size of 5-10 mm and a mud content of 0.4%; the river sand is grade II medium sand, with a fineness modulus of 2.9 and a mud content of 1.6%.

8. The method for preparing a highly wear-resistant concrete according to claim 1, It is characterized in that The mineral powder is S95 grade mineral powder with a specific surface area of ​​450m 2 / kg, and the activity index at 28 days was 95%.

9. The method for preparing a highly wear-resistant concrete according to claim 1, It is characterized in that The water reducer is any one of PCE-102 polycarboxylate water reducer, PCE-101 polycarboxylate water reducer and PCE-103 polycarboxylate water reducer.

10. Highly wear-resistant concrete prepared according to the preparation method according to any one of claims 1 to 9.