A preparation method of high power density, high resistivity and low power consumption manganese zinc ferrite
By doping nano-SiO2 and nano-CaCO3 and controlling the sintering process, the problem of high loss of manganese-zeb ferrite material at high frequencies is solved, and the characteristics of high power density and low power consumption are achieved, which are suitable for high-frequency application scenarios.
Patent Information
- Application Number
- CN202411224026.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-03
AI Technical Summary
It is difficult to prepare high power density and low loss manganese zinc ferrite materials at high frequencies and high magnetic flux density, and the cooling rate during sintering is too fast to affect the material performance.
By doping nano-SiO2 and nano-CaCO3, the CaSiO3 glass phase is generated, the cooling rate and oxygen content are regulated, and combined with the sintering process, the material resistivity and power consumption are reduced.
It realizes high power density, high resistivity, and low power consumption characteristics under 1.5MHz to 2MHz and 100mT conditions, meeting the needs of higher frequency, integration and miniaturization of devices.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnetic materials and relates to a method for preparing high-power density, high-resistivity and low-power consumption manganese-zinc ferrite. Background Art
[0002] As the performance of large chips such as CPU / GPU continues to improve, the power supply requirements are further improved. Large chips including CPU and GPU continue to develop towards higher performance (higher main frequency / greater computing power), and the requirements for their motherboard power supply systems are also getting higher and higher: 1) The high precision of components requires that the power supply voltage be strictly controlled within a certain range; 2) The substantial increase in chip power consumption also leads to a rapid increase in the working current, which places extremely high demands on the high-load performance of the power supply, which requires the power supply core to perform better in conversion efficiency and heat generation, and requires lower core losses. At present, the working conditions of high-frequency and low-power cores in the market are 500kHz~1000kHz, 50~100mT, but with the improvement of the application scenarios and performance requirements of components, new requirements are put forward for ferrite cores for secondary power supplies, requiring the core to be improved in efficiency and loss reduction under the conditions of 1~2MHz and 100mT. Since the loss increases exponentially with the operating frequency and the working magnetic flux density, it is a major challenge to prepare high-power density ferrite and low-loss ferrite.
[0003] The patent with announcement number CN114195500B discloses a wide-temperature, high-frequency, high-magnetic flux density manganese-zinc soft magnetic ferrite for charging piles and its preparation method. It adopts the quaternary main formula technology and combines the secondary sintering technology of the powder to obtain a wide-temperature, low-loss material at 500kHz, 100mT and 1MHz, 100mT. Its application frequency is still relatively low, and the patent does not involve the control of the cooling process during sintering. The patent with announcement number CN100558675C provides a method for preparing a wide-band, low-loss, high-permeability manganese-zinc ferrite material, which involves the cooling process: the cooling rate from 1390℃ to 1000℃ is 150℃ / hour, and the cooling rate from 1000℃ to room temperature is 200℃ / hour. The overall cooling rate is relatively fast, and the patent is simply for temperature control, and does not involve cooperation with the formula to play a role.
[0004] Therefore, in order to meet the device's requirements for high power density and overcome the above difficulties, it is necessary to develop a high-power density, high-resistivity, low-power manganese-zinc ferrite material under the conditions of 1.5MHz~2MHz and 100mT. Summary of the invention
[0005] In order to overcome the deficiencies of the prior art, the present invention provides a method for preparing a manganese-zinc ferrite with high power density, high resistivity and low power consumption, so as to realize the characteristics of high power density, high resistivity and low power consumption of the ferrite material.
[0006] The manganese-zinc ferrite material of the present invention: (1) by doping nano-SiO2 and nano-CaCO3, CaSiO3 is generated by reaction. The glass phase material is distributed at the grain boundary, which can greatly increase the grain boundary resistivity and reduce the eddy current loss of the material; (2) the generation temperature range of the CaSiO3 glass phase is roughly 750-1000°C. In order to further improve the material resistivity, the cooling rate is reduced and the cooling time is extended in the cooling section within this range, so that the liquid phase can be more evenly distributed at the grain boundary, preventing the liquid phase from being enriched at the grain boundary and causing performance deterioration; (3) by controlling the cooling rate and oxygen content, the valence state of the iron and manganese variable valence element ions is regulated to improve the material loss. Through the above doping and sintering process, a manganese-zinc soft magnetic ferrite material with high resistivity and low power consumption at high frequency and high working magnetic flux density is successfully produced.
[0007] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0008] Step 1: Ingredients: weigh the main components, Fe2O3: 55-60mol%, ZnO: 1.0-6.0mol%, and the rest is Mn3O4, and then sand grind and mix;
[0009] Step 2: pre-burning, pre-burning the mixture obtained in step 1;
[0010] Step 3: sand grinding, sieving the pre-burned material obtained in step 2, and then adding auxiliary components and sand grinding again, the auxiliary components are nano-CaCO3, nano-SiO2, Co2O3, Mo2O3, V2O5, Ta2O5, Nb2O5;
[0011] Step 4: Granulation;
[0012] Step 5: Pressing and forming;
[0013] Step 6: sintering, the sintering temperature is 1060-1200°C, the oxygen content in the insulation stage is 1.2-3.2%, and the temperature is lowered after insulation. In the cooling stage from 950-1000°C to 750-800°C, the cooling rate is 10-40°C / h, and the cooling rate in other cooling stages is 60-240°C / h. The other cooling stages are: 1060-1200°C to 950-1000°C cooling stage, and 750-800°C to room temperature cooling stage.
[0014] Preferably, the main components include Fe2O3: 57-59.5 mol%, ZnO: 2.0-5.0 mol%, and the rest is Mn3O4.
[0015] Preferably, the main components include Fe2O3: 58-58.5 mol%, ZnO: 2.5-4.0 mol%, and the rest is Mn3O4.
[0016] Preferably, based on the total weight of the main components, the auxiliary components include: nano-CaCO3: 500-1500ppm, nano-SiO2: 50-150ppm, Co2O3: 1000-2000ppm, Mo2O3: 200-500ppm, V2O5: 200-500ppm, Ta2O5: 200-400ppm, and Nb2O5: 100-300ppm.
[0017] Preferably, based on the total weight of the main components, the nano-CaCO3 content is 700ppm, 900ppm, 1100ppm or 1300ppm; the nano-SiO2 content is 70ppm, 90ppm, 110ppm or 130ppm; the Co2O3 content is 1200ppm, 1400ppm, 1600ppm or 1800ppm; the Mo2O3 content is 250ppm, 300ppm, 350ppm, 400ppm or 450ppm; the V2O5 content is 250ppm, 300ppm, 350ppm, 400ppm or 450ppm; the Ta2O5 content is 250ppm, 300ppm or 350ppm; and the Nb2O5 content is 150ppm, 200ppm or 250ppm.
[0018] Wherein, in step 1, wet sand grinding is adopted for mixing, and the mixing time is 5 to 20 minutes.
[0019] Wherein, in step 2, the mixed material obtained in step 1 is pre-fired in air, the pre-fired temperature is 850-950° C., the heating rate is 3-5° C. / min, and the pre-fired material is sieved through a 40-mesh sieve.
[0020] Wherein, in step 3, the sand grinding time is 30 to 100 min, preferably 40 min, 50 min, 60 min, 70 min, 80 min or 90 min, and the particle size D50 of the powder after sand grinding is 1.0 μm to 1.6 μm.
[0021] Among them, in step 4, granulation is carried out after adding polyvinyl alcohol, the mass fraction of polyvinyl alcohol is 8% to 15%, and after the granulation is completed, it is sieved through a 120-mesh sieve.
[0022] Preferably, in step 6, 950-1000°C may be 950°C, 960°C, 970°C, 980°C, 990°C or 1000°C, and 750-800°C may be 750°C, 760°C, 770°C, 780°C, 790°C or 800°C;
[0023] Preferably, in step 6, in the cooling section from 950-1000°C to 750-800°C, the cooling rate is 15-35°C / h, and the cooling rate in other cooling sections is 70-210°C / h. The other cooling sections are: a cooling section from 1060-1200°C to 950-1000°C and a cooling section from 750-800°C to room temperature.
[0024] Preferably, in step 6, the cooling process of other cooling sections is as follows: in the cooling section from 1060-1200°C to 950-1000°C, the cooling rate is 90-210°C / h; in the cooling section from 750-800°C to 300-400°C, the cooling rate is 90-210°C / h; during the period from 300-400°C to room temperature, the cooling rate is 90-210°C / h.
[0025] Preferably, in step 6, the sintering temperature is 1080-1180°C, the holding time is 3-6h, and the oxygen content in the holding period is 1.5-3.0%; after holding, the temperature is lowered, preferably, in the range of 1080-1180°C to 950-1000°C, the cooling rate is 90-150°C / h, and the oxygen content is reduced to 0.3-0.5%; in the range of 950-1000°C to 750-800°C, the cooling rate is 20-35°C / h, and the oxygen content is reduced to 0.1-0.28%; in the range of 750-800°C to 300-400°C, the cooling rate is 90-180°C / h, and the oxygen content is reduced to 0.05-0.09%; during the period from 300-400°C to room temperature, the cooling rate is 90-180°C / h, and the oxygen content is reduced to below 0.01%.
[0026] Preferably, in step 6, the sintering temperature is 1100-1150°C, the holding time is 3.5-5.5h, and the oxygen content in the holding period is 1.7-2.8%; after holding, the temperature is lowered, preferably, in the range of 1100-1150°C to 950-1000°C, the cooling rate is 100-130°C / h, and the oxygen content is reduced to 0.35-0.45%; in the range of 950-1000°C to 750-800°C, the cooling rate is 25-30°C / h, and the oxygen content is reduced to 0.1-0.2%; in the range of 750-800°C to 300-400°C, the cooling rate is 100-160°C / h, and the oxygen content is reduced to 0.06-0.09%; during the period from 300-400°C to room temperature, the cooling rate is 120-170°C / h, and the oxygen content is reduced to below 0.01%.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] This high-frequency material can be used in application scenarios with high operating frequencies of 1.5MHz to 2MHz and high operating magnetic flux density of 100mT. It also has the characteristics of low power consumption and can meet the needs of higher frequency, integration and miniaturization of devices. DETAILED DESCRIPTION
[0029] The following is a further detailed description of the high power density and low power consumption manganese zinc ferrite material and preparation process prepared by the present invention through specific implementation cases. According to the following preparation method, three manganese zinc ferrite materials in Examples 1 to 3 and three manganese zinc ferrite materials in Comparative Examples 1 to 3 were prepared.
[0030] Example 1 is as follows:
[0031] A method for preparing high power density, high resistivity and low power consumption manganese zinc ferrite comprises the following steps:
[0032] Step 1: Ingredients: Fe2O3, ZnO, and Mn3O4 are weighed in proportion, and the main components are Fe2O3: 59.0mol%, ZnO: 4.5mol%, and MnO: 36.5mol%, respectively, and then wet sand milled and mixed for 10 minutes;
[0033] Step 2: Pre-burning: drying the mixed material obtained in step 1 and pre-burning it in air at a temperature of 880°C and a heating rate of 5°C / min. The pre-burned material is sieved through a 40-mesh sieve;
[0034] Step 3: Sand grinding: add auxiliary components: nano-CaCO3: 1100ppm, nano-SiO2: 110ppm, Co2O3: 1800ppm, Mo2O3: 300ppm, V2O5: 300ppm, Ta2O5: 200ppm, Nb2O5: 150ppm, sand grinding and the sand grinding time is 60min, and the powder particle size D50 after sand grinding is 1.0μm~1.6μm;
[0035] Step 4: Granulation: Dry and granulate the sand-milled slurry, the mass fraction of polyvinyl alcohol is 12%, and sieve through a 120-mesh sieve after granulation;
[0036] Step 5: Pressing: Pressing into a ring-shaped green body with a size of Φ12.7mm×Φ8mm×7mm;
[0037] Step 6: Sintering, the sintering temperature is 1150℃, the holding time is 5.5h, the oxygen content in the holding period is 2.2%, and the temperature is lowered after holding, from 1150℃ to 1000℃, the cooling rate is 120℃ / h, and the oxygen content is reduced to 0.3%; from 1000℃ to 800℃, the cooling rate is 25℃ / h, and the oxygen content is reduced to 0.15%; from 800℃ to 400℃, the cooling rate is 150℃ / h, and the oxygen content is reduced to 0.08%; from 400℃ to room temperature, the cooling rate is 150℃ / h.
[0038] Example 2: The difference from Example 1 is that the main components are Fe2O3: 59.4mol%, ZnO: 4.1mol%, and MnO: 36.5mol%.
[0039] Example 3: The difference from Example 1 is that during the sintering process, in the cooling section from 1000°C to 800°C, the cooling rate is 30°C / h.
[0040] Comparative Example 1: The difference from Example 1 is that the main components are Fe2O3: 57.2 mol%, ZnO: 5.0 mol%, and MnO: 37.8 mol%.
[0041] Comparative Example 2: The difference from Example 2 is that the auxiliary components are non-nanoscale CaCO3: 1100ppm, SiO2: 110ppm.
[0042] Comparative Example 3: The difference from Example 3 is that during the sintering process, the cooling rate in the cooling section from 1000°C to 800°C is 200°C / h.
[0043] Table 1 Comparison of magnetic properties of the embodiment and the comparative example
[0044]
[0045] The material loss was tested under the conditions of 1.5MHz, 100mT and 2MHz, 100mT. Table 1 is a comparison of the magnetic properties of the embodiment and the comparative example. It can be seen from the table that the best magnetic properties are obtained in the manufacturing method of the present invention according to the embodiment 1, 2 and 3. Comparing the comparative example 1 with the embodiment 1, it is found that when the iron content of the main formula is not within the range of the above main formula, the loss increases significantly; comparing the comparative example 2 with the embodiment 2, it is found that when the doped nano-scale calcium oxide and silicon dioxide are replaced with ordinary calcium oxide and silicon dioxide, the loss will deteriorate to a certain extent; comparing the comparative example 3 with the embodiment 3, it is found that after the cooling rate of the cooling section of 1000℃~800℃ is accelerated, the performance deteriorates significantly.
[0046] The above descriptions are only some embodiments of the present invention, but the protection scope of the present invention is not limited thereto.
Claims
1. A method for preparing high power density, high resistivity and low power consumption manganese zinc ferrite. It is characterized in that The following steps are involved: Step 1: Ingredients, weigh the main ingredients, Fe 2 O 3 : 55~60mol%, ZnO: 1.0~6.0mol%, the rest is Mn 3 O 4 , then sand-grind and mix; Step 2: pre-burning, pre-burning the mixture obtained in step 1; Step 3: Sand grinding: the pre-burned material obtained in step 2 is sieved, and then the auxiliary component is added and sand ground again. The auxiliary component is nano-CaCO 3 、Nano-SiO 2 、Co 2 O 3 、Mo 2 O 3 、V 2 O 5 、 2 O 5 , Nb 2 O 5 Among them, nano-CaCO 3 : 500~1500ppm, nano-SiO 2 : 50~150ppm; Step 4: Granulation; Step 5: Pressing and forming; Step 6: sintering, the sintering temperature is 1080-1180°C, the oxygen content in the insulation stage is 1.5-3.0%, and the temperature is lowered after insulation. In the cooling stage from 1080-1180°C to 950-1000°C, the cooling rate is 90-150°C / h, and the oxygen content is reduced to 0.3-0.5%; in the cooling stage from 950-1000°C to 750-800°C, the cooling rate is 20-35°C / h, and the oxygen content is reduced to 0.1-0.28%; in the range from 750-800°C to 300-400°C, the cooling rate is 90-180°C / h, and the oxygen content is reduced to 0.05-0.09%; during the period from 300-400°C to room temperature, the cooling rate is 90-180°C / h, and the oxygen content is reduced to below 0.01%.
2. A method for preparing a high power density, high resistivity and low power consumption manganese zinc ferrite as claimed in claim 1, It is characterized in that The main component includes Fe 2 O 3 : 57~59.5mol%, ZnO: 2.0~5.0mol%, the rest is Mn 3 O 4 .
3. A method for preparing a high power density, high resistivity and low power consumption manganese zinc ferrite as claimed in claim 1, It is characterized in that Calculated by the total weight of the main components, the auxiliary components include: nano-CaCO 3 : 500~1500ppm, nano-SiO 2 :50~150ppm、Co 2 O 3 :1000~2000ppm、Mo 2 O 3 :200~500ppm、V 2 O 5 :200~500ppm、Ta 2 O 5 :200~400ppm、Nb 2 O 5 : 100~300ppm.
4. A method for preparing a high power density, high resistivity and low power consumption manganese zinc ferrite as claimed in claim 1, It is characterized in that In the step 1, wet sand milling is used for mixing, and the mixing time is 5 to 20 minutes; in the step 2, the mixed material obtained in the step 1 is pre-burned in the air, the pre-burning temperature is 850 to 950°C, the heating rate is 3 to 5°C / min, and the pre-burned material is sieved through a 40-mesh sieve; in the step 3, the sand milling time is 30 to 100 minutes, and the particle size D50 of the powder after sand milling is 1.0 μm to 1.6 μm; in the step 4, granulation is carried out after adding polyvinyl alcohol, the mass fraction of polyvinyl alcohol is 8% to 15%, and the granulation is completed and the mixture is sieved through a 120-mesh sieve.
5. A method for preparing a high power density, high resistivity and low power consumption manganese zinc ferrite according to any one of claims 1 to 4, It is characterized in that In step 6, the sintering temperature is 1080-1180° C., the holding time is 3-6 hours, and the oxygen content in the holding section is 1.5-3.0%.
6. A method for preparing a high power density, high resistivity and low power consumption manganese zinc ferrite according to any one of claims 1 to 4, It is characterized in that In step 6, the sintering temperature is 1100-1150° C., the holding time is 3.5-5.5 hours, and the oxygen content in the holding section is 1.7-2.8%.
7. A method for preparing a high power density, high resistivity and low power consumption manganese zinc ferrite as claimed in claim 6, It is characterized in that The entire cooling process after insulation is as follows: from 1100-1150°C to 950-1000°C, the cooling rate is 100-130°C / h, and the oxygen content drops to 0.3-0.5%; from 950-1000°C to 750-800°C, the cooling rate is 25-30°C / h, and the oxygen content drops to 0.1-0.2%; from 750-800°C to 300-400°C, the cooling rate is 100-160°C / h, and the oxygen content drops to 0.06-0.09%; from 300-400°C to room temperature, the cooling rate is 120-170°C / h, and the oxygen content drops to below 0.01%.