A method for synthesizing succinonitrile

The preparation of catalysts by zinc-aluminum hydrotalcite-supported magnesium and cerium and X-type zeolite bentonite has solved the problem of complex or high cost of existing succinitrile synthesis processes, achieved high yield and long-life catalysts, and reduced pollution and production costs. .

CN118724748BActive Publication Date: 2024-11-22YUANCATALYST TECHNOLOGY (SHENYANG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411220682.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-22
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The existing succinitrile synthesis methods are complex in process or high in cost, low in yield, and the catalysts used contain chromium, causing contamination.

Method used

The catalyst is prepared by using zinc-aluminum hydrotalcite-type hydrotalcite-supported active components magnesium and cerium, mixed with X-type zeolite and bentonite for spray granulation and roasting. It is used to react with raw materials and ammonia in the catalyst bed to produce high yield succinitrile .

Benefits of technology

It improves the activity and life of the catalyst, increases the yield of succinitrile, simplifies the process, and reduces pollution and production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of fine chemicals, and specifically relates to a method for synthesizing succinonitrile. The method comprises the following steps: a raw material and ammonia are introduced into a catalyst bed for reaction. The catalyst is prepared by first preparing zinc-aluminum hydrotalcite, then loading active components of magnesium and cerium, and then mixing with X-type zeolite and bentonite, spraying granulation, and roasting to obtain a catalyst. The catalyst used in the present invention has excellent catalytic activity and lifespan. The synthesized succinonitrile has a higher yield by using the catalyst of the present invention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of fine chemicals and more specifically relates to a method for synthesizing succinonitrile. Background Art

[0002] Succinonitrile, also known as 1,2-dicyanoethane and succinonitrile, has a molecular formula of C4H4N2. It is a colorless, odorless waxy substance that is soluble in water, ethanol, and chloroform. Relative density (water = 1) 1.02, relative density (air = 1) 2.1. Relative molecular weight 80.09, melting point 58.1°C, boiling point 267°C. Succinonitrile is an important fine chemical intermediate with a wide range of uses. It is widely used in automobiles and galvanized iron coatings to obtain quinacridone pigments; as well as electrolyte additives to improve the performance of lithium batteries, and can also be used in the production of nylon, etc.

[0003] In industry, there are two main methods for synthesizing succinonitrile: (1) using acrylonitrile as raw material, reacting with hydrocyanic acid under alkaline conditions, and then obtaining it through separation processes such as distillation, with a yield of more than 95% and a content of more than 99.5%; (2) adding 1,2-dibromoethane ethanol solution to a hot sodium cyanide aqueous solution, and reacting it under reflux to generate succinonitrile, and the reaction liquid is separated and distilled to obtain the finished succinonitrile. The above two processes are either complicated or costly with low yield.

[0004] CN115888779A discloses a catalyst for preparing succinonitrile by catalytic amination and a preparation method of succinonitrile. With succinic acid and the like as starting materials, succinonitrile is continuously prepared by one-step reaction in the presence of a catalyst. The preparation method is simple and easy to operate, easy to control, less polluting, high product yield and good quality. The catalyst has good activity and selectivity, stable performance, long service life, high raw material conversion rate, few side reactions, and effectively reduces the production cost and the generation of three wastes. However, the catalyst used in the document contains chromium, and the use of chromium can cause pollution. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide a method for synthesizing succinonitrile. The method comprises the following steps: introducing raw materials and ammonia into a catalyst bed for reaction. The catalyst is prepared by first preparing zinc-aluminum hydrotalcite, then loading active components of magnesium and cerium, then mixing with X-type zeolite and bentonite, spray granulation, and roasting to obtain the catalyst. The catalyst used in the present invention has excellent catalytic activity and lifespan. The synthesized succinonitrile has a higher yield by using the catalyst of the present invention.

[0006] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0007] A method for synthesizing succinonitrile, the method comprising the following steps:

[0008] The raw materials and ammonia gas are introduced into the catalyst bed for reaction.

[0009] The preferred technical solution is that the method for preparing the catalyst comprises the following steps:

[0010] (1) Weighing zinc salt and aluminum salt and ultrasonically dispersing them in deionized water to prepare a mixed salt solution, then dropping alkali solution to adjust the pH of the solution, then transferring the solution to a hydrothermal reactor for reaction, centrifuging, washing, drying, and grinding to obtain a hydrotalcite-like substance;

[0011] (2) Add the hydrotalcite-like substance, magnesium salt and cerium salt obtained in step (1) to deionized water, stir evenly, then add alkali solution dropwise to adjust the pH value of the solution to 11, let stand for 8-12 hours, filter, wash, and dry at 80-120° C. for 8-12 hours to obtain product A. Grind the obtained product A, X-type zeolite, bentonite and an appropriate amount of water to obtain a slurry, then spray granulate, and calcine at 500-600° C. for 4-10 hours to obtain a catalyst.

[0012] Preferably, in step (1), the pH is 9-11; and the hydrothermal reaction is carried out at 110-150° C. for 10-28 hours.

[0013] Further preferably, in step (1), the drying is vacuum drying at 60-80° C. for 14-20 h; the zinc salt is at least one of zinc nitrate, zinc acetate, and zinc chloride; and the aluminum salt is at least one of aluminum acetate, aluminum chloride, and aluminum nitrate.

[0014] More preferably, in step (1), the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.3-0.5.

[0015] More preferably, in step (1), the molar ratio of the zinc salt to the aluminum salt is 2-3:1, and the concentration of the alkali solution is 3-5 mol / L.

[0016] Preferably, in step (2), the ratio of the hydrotalcite-like substance, magnesium salt and cerium salt obtained in step (1) is: 100 g: 0.02-0.04 mol: 0.01-0.03 mol; the alkali is sodium hydroxide or potassium hydroxide, and the concentration of the alkali is 2-4 mol / L.

[0017] Further preferably, in step (2), the magnesium salt is at least one of magnesium nitrate, magnesium acetate and magnesium chloride; the cerium salt is at least one of cerium nitrate, cerium acetate and cerium chloride; and the mass ratio of the product A, X-type zeolite and bentonite is 0.6~1:0.2~0.6:1.

[0018] The preferred technical solution is that the raw material is succinic acid, succinic anhydride or dimethyl succinate; the reaction conditions are that the molar ratio of the raw material to ammonia is 1:2-20; the reaction pressure is 0.1-5 MPa, and the raw material space velocity is 0.1-1.5 h -1 ; The reaction temperature is 350~450℃.

[0019] According to a preferred technical solution, the raw material is preheated before entering the catalyst bed together with ammonia, and the preheating temperature is 180-220°C.

[0020] In the present invention, a preferred technical solution is a method for synthesizing succinonitrile, the method comprising the following steps:

[0021] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0022] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0023] S3, after the raw materials are metered, they enter the preheating section through the feeder, and after preheating, they enter the catalyst bed together with ammonia gas to react;

[0024] S4. The crude product is purified by distillation to obtain the product succinonitrile.

[0025] The present invention has the following beneficial effects:

[0026] (1) Zinc-aluminum hydrotalcite is used as a carrier to load active components of magnesium and cerium, so that the catalyst of the present invention has excellent activity and selectivity, thereby affecting the yield of succinonitrile;

[0027] (2) The catalyst was mixed with X-type zeolite and bentonite, spray granulated, and calcined to further improve the catalyst yield and life.

[0028] (3) The preparation process of the catalyst of the present invention is simple and has good process prospects. DETAILED DESCRIPTION

[0029] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0030] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0031] Example 1

[0032] A method for synthesizing succinonitrile, the method comprising the following steps:

[0033] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0034] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0035] S3, after being metered, succinic acid enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 200°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:12; the reaction pressure is 2Mpa, and the raw material space velocity is 1h -1 ; The reaction temperature is 400℃.

[0036] S4. The crude product is purified by distillation to obtain the product succinonitrile, wherein the yield of succinonitrile is 99.5% and the catalyst life is 2750h.

[0037] The method for preparing the catalyst comprises the following steps:

[0038] (1) Weigh 2.5 mol zinc nitrate and 1 mol aluminum chloride and ultrasonically disperse them in 250 mL deionized water to prepare a mixed salt solution, then drop 4 mol / L alkali solution (the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.4) to adjust the pH of the solution to 10, then transfer to a hydrothermal reactor and react at 130°C for 20 hours, centrifuge, wash, vacuum dry at 70°C for 18 hours, and grind to obtain a hydrotalcite-like substance;

[0039] (2) 100 g of the hydrotalcite obtained in step (1), 0.03 mol of magnesium nitrate and 0.02 mol of cerium acetate were added to 200 mL of deionized water and stirred evenly. Then, a 3 mol / L sodium hydroxide solution was added dropwise to adjust the pH of the solution to 11. The solution was allowed to stand for 10 h, filtered, washed and dried at 100 °C for 10 h to obtain product A. 80 g of product A, 40 g of X-type zeolite, 100 g of bentonite and an appropriate amount of water were ground evenly to obtain a slurry, which was then spray granulated and calcined at 550 °C for 6 h to obtain a catalyst.

[0040] Example 2

[0041] A method for synthesizing succinonitrile, the method comprising the following steps:

[0042] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0043] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0044] S3, after being metered, succinic anhydride enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 220°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:18; the reaction pressure is 0.2Mpa, and the raw material space velocity is 1.4h-1 ; The reaction temperature is 440℃.

[0045] S4. The crude product is purified by distillation to obtain the product succinonitrile, wherein the yield of succinonitrile is 99.1% and the catalyst life is 2725h.

[0046] The preparation method of the catalyst comprises the following steps:

[0047] (1) Weigh 3 mol of zinc acetate and 1 mol of aluminum nitrate and ultrasonically disperse them in 250 mL of deionized water to prepare a mixed salt solution, then dropwise add 4 mol / L alkali solution (the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.4) to adjust the pH of the solution to 11, then transfer to a hydrothermal reactor and react at 150° C. for 10 h, centrifuge, wash, vacuum dry at 80° C. for 14 h, and grind to obtain a hydrotalcite-like substance;

[0048] (2) 100 g of the hydrotalcite obtained in step (1), 0.04 mol of magnesium acetate and 0.01 mol of cerium chloride were added to 200 mL of deionized water and stirred evenly. Then, a 4 mol / L potassium hydroxide solution was added dropwise to adjust the pH of the solution to 11. The solution was allowed to stand for 12 h, filtered, washed and dried at 120 ° C for 8 h to obtain product A. 100 g of product A, 20 g of X-type zeolite, 100 g of bentonite and an appropriate amount of water were ground evenly to obtain a slurry, which was then spray granulated and calcined at 600 ° C for 4 h to obtain a catalyst.

[0049] Example 3

[0050] A method for synthesizing succinonitrile, the method comprising the following steps:

[0051] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0052] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0053] S3, dimethyl succinate is metered and enters the preheating section through the feeder, and after preheating, it enters the catalyst bed together with ammonia to react; the preheating temperature is 180°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:4; the reaction pressure is 4.8Mpa, and the raw material space velocity is 0.2h -1 ; The reaction temperature is 360℃.

[0054] S4. The crude product is purified by distillation to obtain the product succinonitrile, wherein the yield of succinonitrile is 98.8% and the catalyst life is 2740h.

[0055] The preparation method of the catalyst comprises the following steps:

[0056] (1) Weigh 2 mol of zinc chloride and 1 mol of aluminum acetate and ultrasonically disperse them in 250 mL of deionized water to prepare a mixed salt solution, then dropwise add 4 mol / L alkali solution (the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.4) to adjust the pH of the solution to 9, then transfer to a hydrothermal reactor and react at 110° C. for 28 h, centrifuge, wash, vacuum dry at 60° C. for 20 h, and grind to obtain a hydrotalcite-like substance;

[0057] (2) Add 100 g of the hydrotalcite-like substance obtained in step (1), 0.02 mol of magnesium chloride and 0.03 mol of cerium nitrate to 200 mL of deionized water and stir evenly, wherein the ratio of the hydrotalcite-like substance obtained in step (1), magnesium salt and cerium salt is: 100 g: 0.02 mol: 0.03 mol; then add dropwise a 2 mol / L sodium hydroxide solution to adjust the pH value of the solution to 11, let stand for 8 h, filter, wash and dry at 80° C. for 12 h to obtain product A, grind 60 g of product A, 60 g of X-type zeolite, 100 g of bentonite and an appropriate amount of water to obtain a slurry, spray granulate and calcine at 500° C. for 10 h to obtain a catalyst.

[0058] Comparative Example 1

[0059] A method for synthesizing succinonitrile, the method comprising the following steps:

[0060] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0061] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0062] S3, after being metered, succinic acid enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 200°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:12; the reaction pressure is 2Mpa, and the raw material space velocity is 1h -1 ; The reaction temperature is 400℃.

[0063] S4, the crude product is purified by rectification to obtain the product succinonitrile, wherein the yield of succinonitrile is 97.3%.

[0064] The method for preparing the catalyst comprises the following steps:

[0065] (1) Same as step (1) of Example 1;

[0066] (2) Add 100 g of the hydrotalcite obtained in step (1) and 0.05 mol of magnesium nitrate to 200 mL of deionized water, stir evenly, then add dropwise a 3 mol / L sodium hydroxide solution to adjust the solution to a pH of 11; let stand for 10 h, filter, wash, and dry at 100 °C for 10 h to obtain product A; grind 80 g of product A, 40 g of X-type zeolite, 100 g of bentonite and an appropriate amount of water to obtain a slurry, then spray granulate, and calcine at 550 °C for 6 h to obtain a catalyst.

[0067] Comparative Example 2

[0068] A method for synthesizing succinonitrile, the method comprising the following steps:

[0069] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0070] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0071] S3, after being metered, succinic acid enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 200°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:12; the reaction pressure is 2Mpa, and the raw material space velocity is 1h -1 ; The reaction temperature is 400℃.

[0072] S4, the crude product is purified by rectification to obtain the product succinonitrile, wherein the yield of succinonitrile is 96.8%.

[0073] The method for preparing the catalyst comprises the following steps:

[0074] (1) Same as step (1) of Example 1;

[0075] (2) 100 g of the hydrotalcite obtained in step (1) and 0.05 mol of cerium acetate were added to 200 mL of deionized water and stirred evenly. Then, a 3 mol / L sodium hydroxide solution was added dropwise to adjust the pH of the solution to 11. The solution was allowed to stand for 10 h, filtered, washed, and dried at 100 °C for 10 h to obtain product A. 80 g of product A, 40 g of X-type zeolite, 100 g of bentonite and an appropriate amount of water were ground evenly to obtain a slurry, which was then spray granulated and calcined at 550 °C for 6 h to obtain a catalyst.

[0076] Comparative Example 3

[0077] A method for synthesizing succinonitrile, the method comprising the following steps:

[0078] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0079] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0080] S3, after being metered, succinic acid enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 200°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:12; the reaction pressure is 2Mpa, and the raw material space velocity is 1h -1 ; The reaction temperature is 400℃.

[0081] S4. The crude product is purified by distillation to obtain the product succinonitrile, wherein the yield of succinonitrile is 98.2% and the catalyst life is 2130h.

[0082] The method for preparing the catalyst comprises the following steps:

[0083] (1) Same as step (1) of Example 1;

[0084] (2) Add 100 g of the hydrotalcite obtained in step (1), 0.03 mol of magnesium nitrate and 0.02 mol of cerium acetate to 200 mL of deionized water and stir evenly. Then, add dropwise a 3 mol / L sodium hydroxide solution to adjust the solution to a pH of 11. Let stand for 10 h, filter, wash and dry at 100 °C for 10 h to obtain product A. Grind 80 g of product A, 140 g of X-type zeolite and an appropriate amount of water to obtain a slurry. Then, spray granulate the slurry and calcine at 550 °C for 6 h to obtain a catalyst.

[0085] Comparative Example 4

[0086] A method for synthesizing succinonitrile, the method comprising the following steps:

[0087] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0088] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0089] S3, after being metered, succinic acid enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 200°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:12; the reaction pressure is 2Mpa, and the raw material space velocity is 1h -1 ; The reaction temperature is 400℃.

[0090] S4. The crude product is purified by distillation to obtain the product succinonitrile, wherein the yield of succinonitrile is 97.5% and the catalyst life is 2710h.

[0091] The method for preparing the catalyst comprises the following steps:

[0092] (1) Same as step (1) of Example 1;

[0093] (2) Add 100 g of the hydrotalcite obtained in step (1), 0.03 mol of magnesium nitrate and 0.02 mol of cerium acetate to 200 mL of deionized water and stir evenly. Then, add dropwise 3 mol / L sodium hydroxide solution to adjust the pH of the solution to 11. Let stand for 10 h, filter, wash and dry at 100 °C for 10 h to obtain product A. Grind 80 g of product A, 140 g of bentonite and an appropriate amount of water to obtain a slurry. Then, spray granulate the slurry and calcine at 550 °C for 6 h to obtain a catalyst.

[0094] Comparative Example 5

[0095] A method for synthesizing succinonitrile, the method comprising the following steps:

[0096] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0097] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0098] S3, after being metered, succinic acid enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 200°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:12; the reaction pressure is 2Mpa, and the raw material space velocity is 1h -1 ; The reaction temperature is 400℃.

[0099] S4. The crude product is purified by distillation to obtain the product succinonitrile, wherein the yield of succinonitrile is 73.6% and the catalyst life is 2640h.

[0100] The method for preparing the catalyst comprises the following steps:

[0101] 120 g of X-type zeolite, 100 g of bentonite and an appropriate amount of water were ground evenly to obtain a slurry, which was then spray-granulated and calcined at 550° C. for 6 h to obtain a catalyst.

[0102] Comparative Example 6

[0103] A method for synthesizing succinonitrile, the method comprising the following steps:

[0104] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0105] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0106] S3, after being metered, succinic acid enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 200°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:12; the reaction pressure is 2Mpa, and the raw material space velocity is 1h -1 ; The reaction temperature is 400℃.

[0107] S4. The crude product is purified by distillation to obtain the product succinonitrile, wherein the yield of succinonitrile is 98.5% and the catalyst life is 2750h.

[0108] The method for preparing the catalyst comprises the following steps:

[0109] (1) Same as step (1) of Example 1;

[0110] (2) Add 100 g of the hydrotalcite obtained in step (1), 0.03 mol of magnesium nitrate and 0.02 mol of cerium acetate to 200 mL of deionized water and stir evenly. Then, add dropwise 3 mol / L sodium hydroxide solution to adjust the pH of the solution to 11. Let stand for 10 h, filter, wash and dry at 100 °C for 10 h to obtain product A. Grind 120 g of product A, 100 g of bentonite and an appropriate amount of water to obtain a slurry. Then, spray granulate the slurry and calcine at 550 °C for 6 h to obtain a catalyst.

[0111] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for synthesizing succinonitrile, characterized in that: The method comprises the following steps: The raw materials and ammonia are introduced into the catalyst bed for reaction; The raw material is succinic acid, succinic anhydride or dimethyl succinate; the reaction conditions are that the molar ratio of the raw material to ammonia is 1:2-20; the reaction pressure is 0.1-5 MPa, and the raw material space velocity is 0.1-1.5 h -1 ; Reaction temperature is 350~450℃; The preparation method of the catalyst comprises the following steps: (1) Weigh zinc salt and aluminum salt and ultrasonically disperse them in deionized water to prepare a mixed salt solution, then drop alkali solution to adjust the pH of the solution, then transfer the solution to a hydrothermal reactor for reaction, centrifuge, wash, dry, and grind to obtain a hydrotalcite-like substance; the molar ratio of the zinc salt to the aluminum salt is 2-3:1: (2) Add the hydrotalcite-like substance, magnesium salt and cerium salt obtained in step (1) to deionized water, stir evenly, then add alkali solution dropwise to adjust the pH value of the solution to 11, let stand for 8-12 hours, filter, wash, and dry at 80-120°C for 8-12 hours to obtain product A, grind the obtained product A, X-type zeolite, bentonite and an appropriate amount of water evenly to obtain a slurry, then spray granulate, and calcine at 500-600°C for 4-10 hours to obtain a catalyst; the ratio of the hydrotalcite-like substance, magnesium salt and cerium salt obtained in step (1) is: 100g: 0.02-0.04mol: 0.01-0.03mol; the mass ratio of the product A, X-type zeolite and bentonite is: 0.6-1:0.2-0.6:

1.

2. A method for synthesizing succinonitrile according to claim 1, characterized in that: In step (1), the pH is 9-11; and the hydrothermal reaction is carried out at 110-150° C. for 10-28 hours.

3. A method for synthesizing succinonitrile according to claim 1, characterized in that: In step (1), the drying is vacuum drying at 60-80° C. for 14-20 hours; the zinc salt is at least one of zinc nitrate, zinc acetate, and zinc chloride; and the aluminum salt is at least one of aluminum acetate, aluminum chloride, and aluminum nitrate.

4. A method for synthesizing succinonitrile according to claim 1, characterized in that: In step (1), the alkali in the alkali solution is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.3-0.

5.

5. A method for synthesizing succinonitrile according to claim 1, characterized in that: In step (1), the concentration of the alkali solution is 3-5 mol / L.

6. A method for synthesizing succinonitrile according to claim 1, characterized in that: In step (2), the alkali in the alkali solution is sodium hydroxide or potassium hydroxide, and the concentration of the alkali is 2-4 mol / L.

7. A method for synthesizing succinonitrile according to claim 1, characterized in that: In step (2), the magnesium salt is at least one of magnesium nitrate, magnesium acetate, and magnesium chloride; the cerium salt is at least one of cerium nitrate, cerium acetate, and cerium chloride.

8. A method for synthesizing succinonitrile according to claim 1, characterized in that: The raw material is preheated before entering the catalyst bed together with ammonia, and the preheating temperature is 180-220°C.