Disubstituted phosphinate compound as well as preparation method and application thereof
The one-step synthesis of disubstituted phosphinate and epoxy resin solves the existing problems of complicated processes and difficulty in achieving transparent flame retardancy, and achieves a highly efficient and low-cost transparent flame retardant epoxy resin cured product, which is suitable for Electronic components and new energy fields.
Patent Information
- Application Number
- CN202410768959.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The existing synthesis process of disubstituted phosphinates is complex, costly, polluted by by-products, and difficult to achieve transparent flame-retardant modification of epoxy resin, which limits its application in the fields of electronic components and new energy.
Disubstituted phosphinates are synthesized in one step using phosphinates and halogenated compounds. By mixing with epoxy resin, acid anhydride curing agent and tertiary amine accelerator, a flame retardant ring with excellent flame retardant properties and transparent properties is prepared. Oxygen resin cured product.
Achieve high-yield, low-cost, environmentally friendly synthesis of disubstituted phosphinates, and prepare transparent and clear flame-retardant epoxy resin cured products, which significantly improve the flame-retardant effect and physical properties, and are suitable for electronic components and new energy fields .
Smart Images

Figure CN118724947A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic phosphorus flame retardants, and in particular to a disubstituted phosphinate compound and a preparation method and application thereof. Background Art
[0002] With the progress and development of society, synthetic polymer materials are widely used in production and life. Because polymer materials are rich in carbon and hydrogen elements, they are very easy to burn. So far, fires caused by the combustion of polymer materials have brought great losses to people. Phosphate ester is a multi-purpose chemical product, among which phosphite and alkyl phosphate are the main varieties of organophosphorus flame retardants, which have the advantages of lasting flame retardant effect, good compatibility with polymer substrates, water resistance, weather resistance, etc., and are widely used in polymer materials such as polyurethane, epoxy resin, polycarbonate, and unsaturated resin. In addition, due to the presence of hypophosphorous acid structure in the molecular structure of disubstituted phosphinate, it also has good flame retardant properties, and disubstituted phosphinate does not contain a monoalkyl structure, does not belong to the international chemical weapons organization monitoring chemicals, and has broad prospects in subsequent development. In the prior art, the synthesis process of disubstituted phosphinate is long, the process is cumbersome, the reaction pressure is high, the equipment requirements are high, the monomers used are expensive, the cost is high, and a large amount of highly polluting halogen acid and flammable and explosive organic matter are produced as byproducts, and the process is not environmentally friendly and unsafe. Therefore, it is necessary to develop a new disubstituted phosphinate synthesis process to solve the problems faced by the existing process.
[0003] In addition, epoxy resin is widely used in the bonding and potting of electronic components due to its excellent performance, and is also used in the preparation and bonding of new energy industry components. However, the low oxygen index of epoxy resin cured products determines that it is a flammable substance, so the application scenario requires it to be flame-retardant modified accordingly. At present, the transparent flame-retardant modification of epoxy resin is still difficult to achieve, which limits its further application development to a certain extent. The flame-retardant modification of epoxy resin in the prior art is mainly based on the addition of powder flame retardants, but the powder can only be dispersed in the epoxy resin and cannot be transparent; if only the industrialized liquid phosphate flame retardant is added, a certain degree of transparency can be achieved, but the compatibility of phosphorus-containing liquid phosphate flame retardants with epoxy resin is not good. During the curing process of epoxy resin, this type of flame retardant will migrate to the surface to form a foggy surface, affecting the appearance and transparency, and it is still difficult to obtain a good flame retardant effect by adding a large amount of this type of phosphate alone. The addition of a large amount of liquid phosphate will have a significant impact on the curing efficiency and softening point of epoxy resin cured products, directly affecting its physical properties. If a flame retardant that can make epoxy resin transparent and flame retardant and is a simple additive type can be prepared, when used for potting electronic components and preparing structural parts, the internal structure can be visually seen, and faults and defects can be discovered in time, which will be conducive to timely solving problems and avoiding more serious consequences. Summary of the invention
[0004] The purpose of the present invention is to provide a disubstituted phosphinate compound and a preparation method and application thereof. The disubstituted phosphinate compound provided by the present invention has excellent flame retardant properties, and is synthesized in a one-step method using phosphinate and halogenated compounds as raw materials. Compared with the existing traditional synthesis method, the method has high yield, few by-products and is easy to separate, simple process, short time consumption, safe and environmentally friendly process, low cost, and easier implementation. The flame-retardant epoxy resin cured product prepared using the disubstituted phosphinate compound as a raw material has excellent flame retardant properties and is transparent and clear.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a disubstituted phosphinate compound having a structure shown in Formula I:
[0007]
[0008] In the formula I: R1, R2, R3 and R4 are independently selected from hydrogen, C1-C8 alkyl, cycloalkyl, aryl or alkenyl, and n is an integer from 1 to 3.
[0009] The present invention also provides a method for preparing the disubstituted phosphinate compound described in the above technical solution, comprising the following steps:
[0010] A phosphinate having a structure of formula II, a halogenated compound having a structure of formula III, an organic solvent and a catalyst are mixed, and then a substitution reaction is carried out in an inert atmosphere to obtain a disubstituted phosphinate;
[0011]
[0012] In the formula II, R1 and R2 are independently selected from hydrogen, C1-C8 alkyl, cycloalkyl, aryl or alkenyl, and M is a metal ion;
[0013] In the formula III, R3 and R4 are independently selected from hydrogen, C1-C8 alkyl, cycloalkyl, aryl or alkenyl, X is a halogen atom, and n is an integer from 1 to 3.
[0014] Preferably, the organic solvent is one or more of toluene, xylene, dioxane, acetonitrile and tetrahydrofuran.
[0015] Preferably, the catalyst is at least one of a phase transfer catalyst and an amphoteric compound.
[0016] The present invention also provides the use of the disubstituted phosphinate compound described in the above technical solution or the disubstituted phosphinate compound prepared by the preparation method in preparing a flame-retardant epoxy resin cured product.
[0017] Preferably, the method for preparing the flame retardant epoxy resin cured product comprises the following steps:
[0018] After the disubstituted phosphinate compound and the epoxy resin are mixed, an acid anhydride curing agent and a tertiary amine accelerator are added to perform curing to obtain a flame retardant epoxy resin cured product.
[0019] Preferably, the mass of the disubstituted phosphinate compound is 7% to 45% of the mass of the epoxy resin.
[0020] Preferably, the acid anhydride curing agent is at least one of methyltetrahydrophthalic anhydride and methylhexahydrophthalic anhydride.
[0021] Preferably, the tertiary amine accelerator is at least one of triethylamine, triethylhydroxylamine, dimethylaminomethylphenol and tris(dimethylaminomethyl)phenol.
[0022] Preferably, the curing temperature is 110° C. to 170° C., and the curing time is 1 to 4 hours.
[0023] The present invention provides a disubstituted phosphinate compound having a structure shown in a specific formula I:
[0024]
[0025] In the formula I: R1, R2, R3 and R4 are independently selected from hydrogen, C1-C8 alkyl, cycloalkyl, aryl or alkenyl, and n is an integer from 1 to 3. The disubstituted phosphinate compound provided by the present invention has excellent flame retardant properties, and it is synthesized in a one-step method using phosphinate and halogenated compounds as raw materials. Compared with the existing traditional synthesis method, it has high yield, few by-products and is easy to separate, simple process, short time consumption, safe and environmentally friendly process, low cost, and easier implementation. The flame-retardant epoxy resin cured product prepared using the disubstituted phosphinate compound as a raw material has excellent flame retardant properties and is transparent and clear. The results of the embodiment show that the flame-retardant epoxy resin cured product test pieces prepared in application examples 1 to 3 of the present invention have significantly better flame retardant effects than those in comparative examples 1 to 2, and the flame-retardant epoxy resin cured products prepared in application examples 1 to 3 are all clear and transparent with better physical properties. It is shown that by using the disubstituted hypophosphite compound provided by the present invention as a flame retardant, a transparent and clear flame-retardant epoxy resin cured product with excellent flame retardancy can be prepared, the transparency of the flame-retardant epoxy resin cured product is achieved, and at the same time, the adverse effects on the physical properties of the flame-retardant foamed polyurethane material are reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the disubstituted phosphinate compound prepared in Example 1 of the present invention;
[0027] Figure 2 This is the P-NMR spectrum of the disubstituted phosphinate compound prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] In the present invention, unless otherwise specified, the raw materials used are conventional commercial products in the art.
[0029] The present invention provides a disubstituted phosphinate compound having a structure shown in Formula I:
[0030]
[0031] In the formula I: R1, R2, R3 and R4 are independently selected from hydrogen, C1-C8 alkyl, cycloalkyl, aryl or alkenyl, and n is an integer from 1 to 3.
[0032] The present invention also provides a method for preparing the disubstituted phosphinate compound described in the above technical solution, comprising the following steps:
[0033] A phosphinate having a structure of formula II, a halogenated compound having a structure of formula III, an organic solvent and a catalyst are mixed, and then a substitution reaction is carried out in an inert atmosphere to obtain a disubstituted phosphinate;
[0034]
[0035] In the formula II, R1 and R2 are independently selected from hydrogen, C1-C8 alkyl, cycloalkyl, aryl or alkenyl, and M is a metal ion;
[0036] In the formula III, R3 and R4 are independently selected from hydrogen, C1-C8 alkyl, cycloalkyl, aryl or alkenyl, X is a halogen atom, and n is an integer from 1 to 3.
[0037] In the present invention, in the formula II, the R1 is preferably one of ethyl, phenyl, propyl, isopropyl, butyl, cyclopropyl, and cyclopentyl; the R2 is preferably at least one of ethyl, phenyl, propyl, isopropyl, butyl, cyclopropyl, and cyclopentyl; and the M is preferably at least one of sodium ion and potassium ion. In the present invention, in the formula III, the R3 is preferably one of hydrogen, methyl, ethyl, and cyclopropyl; the R4 is preferably at least one of ethyl, phenyl, cyclopropane, and cyclopentyl; and the X is preferably a chlorine atom. In the present invention, the molar ratio of the phosphinate having the structure of formula II to the halogenated compound having the structure of formula III is preferably 1:(0.8-2.5), more preferably 1:(1-2, and further preferably 1:1.6.
[0038] In the present invention, the organic solvent is preferably one or more of toluene, xylene, dioxane, acetonitrile, and tetrahydrofuran; the catalyst is at least one of a phase transfer catalyst and an amphoteric compound, more preferably at least one of an ionic polyalkyl quaternary ammonium salt compound, a cationic halogenated polyalkyl quaternary ammonium salt compound, an alkyl ammonium chloride, an alkyl ammonium bromide, an anionic alkyl sulfate compound, an alkyl sulfonate, an alkyl benzene sulfonate, a nonionic surfactant, and a quaternary phosphonium salt, more preferably at least one of 15-Crown-5, 18-crown-6, and tetrabutylammonium bromide. In the present invention, the mass of the catalyst is preferably 2 to 7% of the mass of the phosphinate having the structure of formula II, more preferably 5%.
[0039] In the present invention, the inert atmosphere is preferably nitrogen protection; the substitution reaction is preferably heated under reflux for 8 to 18 hours.
[0040] After the substitution reaction is completed, the product of the substitution reaction is preferably cooled, extracted, dried and rotary evaporated in sequence to obtain a disubstituted phosphinate compound.
[0041] In the present invention, the extraction is preferably performed by adding water and ethyl acetate to the cooled product for extraction. The present invention has no particular limitation on the drying method, and the water in the organic phase obtained by extraction can be removed by using a technical solution well known in the art. The present invention has no particular limitation on the rotary evaporation method, and the organic solvent in the dried product can be removed by rotary drying using a technical solution well known in the art.
[0042] The present invention also provides the use of the disubstituted phosphinate compound described in the above technical solution or the disubstituted phosphinate compound prepared by the preparation method in preparing a flame-retardant epoxy resin cured product.
[0043] In the present invention, the method for preparing the flame retardant epoxy resin cured product preferably comprises the following steps:
[0044] After the disubstituted phosphinate compound and the epoxy resin are mixed, an acid anhydride curing agent and a tertiary amine accelerator are added to perform curing to obtain a flame retardant epoxy resin cured product.
[0045] In the present invention, the mass of the disubstituted phosphinate compound is preferably 7% to 45% of the mass of the epoxy resin, and more preferably 10% to 40%; the epoxy resin is preferably at least one of liquid epoxy resin E51, water-based epoxy resin, two-component epoxy resin, and single-component epoxy resin; the acid anhydride curing agent is preferably at least one of methyltetrahydrophthalic anhydride and methylhexahydrophthalic anhydride; the tertiary amine accelerator is preferably at least one of triethylamine, triethylhydroxylamine, dimethylaminomethylphenol, and tris(dimethylaminomethyl)phenol.
[0046] In the present invention, the curing temperature is preferably 110° C. to 170° C., and the curing time is preferably 1 to 4 hours.
[0047] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] Example 1
[0049] The disubstituted phosphinate compound has the structure shown in Formula I-1:
[0050]
[0051] The preparation method of the disubstituted phosphinate compound having the structure shown in Formula I-1 comprises the following steps:
[0052] 300 mL of toluene, 100 g of 1-chloro-3-cyclopropane-2-propanol, 77 g of diethylphosphite and 3.8 g of 15-Crown-5 were added to a reaction kettle, nitrogen was introduced after mixing, and the mixture was heated to reflux for substitution reaction for 14 h. After the reaction was complete, the mixture was cooled, and water and ethyl acetate were added for extraction. The organic phases were combined, dried and concentrated in turn, and then spin-dried to obtain 88 g of a light yellow oily liquid, i.e., a disubstituted phosphinate compound having the structure shown in Formula I-1, with a yield of 75%.
[0053] The molar ratio of the diethyl hypophosphite to 1-chloro-3-cyclopropane-2-propanol is 1:1.6; the mass of the catalyst 15-Crown-5 is 5.0% of the mass of the diethyl hypophosphite.
[0054] Figure 1 The nuclear magnetic resonance hydrogen spectrum of the disubstituted phosphinate compound prepared in Example 1 of the present invention is Figure 1 It can be seen that 0.6 to 0.9 ppm and 1.39 to 1.59 ppm are the peaks of the methyl group and ethyl group of the ethyl group of the disubstituted phosphinate compound, respectively. Figure 2 The P-NMR spectrum of the disubstituted phosphinate compound prepared in Example 1 of the present invention is shown in FIG. Figure 2 It can be seen that there is a single main peak in the P-NMR spectrum and no splitting occurs, indicating that there is a phosphorus atom in a single chemical environment in the disubstituted phosphinate compound molecule, indicating that Example 1 of the present invention successfully prepared a disubstituted phosphinate compound having the structure shown in Formula I-1.
[0055] Example 2
[0056] A method for preparing a disubstituted phosphinate compound having a structure shown in formula I-1, comprising the following steps: adding 300 mL of toluene, 100 g of 1-chloro-3-cyclopropane-2-propanol, 77 g of diethylphosphite and 3.8 g of tetrabutylammonium bromide into a reaction kettle, introducing nitrogen after mixing, heating to reflux state for substitution reaction for 14 h, cooling after the reaction is complete, adding water and ethyl acetate for extraction, combining the organic phases, drying, concentrating and spin drying to obtain 90 g of a yellow oily liquid with a yield of 77%;
[0057] The molar ratio of the diethyl hypophosphite to 1-chloro-3-cyclopropane-2-propanol is 1:1.6; the mass of the catalyst tetrabutylammonium bromide is 5% of the mass of the diethyl hypophosphite.
[0058] Example 3
[0059] A method for preparing a disubstituted phosphinate compound having a structure shown in formula I-1, comprising the following steps: adding 300 mL of toluene, 100 g of 1-chloro-3-cyclopropane-2-propanol, 77 g of diethylphosphite and 3.8 g of 18-crown-6 into a reaction kettle, introducing nitrogen, heating to reflux for a substitution reaction for 14 h, cooling after the reaction is complete, adding water and ethyl acetate for extraction, combining the organic phases, drying, concentrating and spinning to obtain 94 g of a yellow oily liquid with a yield of 80%;
[0060] The molar ratio of the diethyl hypophosphite to 1-chloro-3-cyclopropane-2-propanol is 1:1.6; the mass of the catalyst 18-crown-6 is 5% of the mass of the diethyl hypophosphite.
[0061] Example 4
[0062] A method for preparing a disubstituted phosphinate compound having a structure shown in formula I-1, comprising the following steps: adding 300 mL of 1,4-dioxane, 100 g of 1-chloro-3-cyclopropane-2-propanol, 77 g of diethylphosphite and 3.8 g of 18-crown-6 to a reaction kettle, introducing nitrogen, heating to reflux for a substitution reaction for 14 h, cooling after the reaction is complete, adding water and ethyl acetate for extraction, combining the organic phases, drying, concentrating and spinning to obtain 71 g of a light yellow oily liquid with a yield of 60%;
[0063] The molar ratio of the diethyl hypophosphite to 1-chloro-3-cyclopropane-2-propanol is 1:1.6; the mass of the catalyst 18-crown-6 is 5% of the mass of the diethyl hypophosphite.
[0064] Example 5
[0065] A method for preparing a disubstituted phosphinate compound having a structure shown in formula I-1, comprising the following steps: adding 300 mL of tetrahydrofuran, 100 g of 1-chloro-3-cyclopropane-2-propanol, 77 g of diethylphosphite and 3.8 g of 18-crown-6 to a reaction kettle, introducing nitrogen, heating to reflux for a substitution reaction for 14 h, cooling after the reaction is complete, adding water and ethyl acetate for extraction, combining the organic phases, drying, concentrating and spin drying to obtain 47 g of a yellow oily liquid with a yield of 41%;
[0066] The molar ratio of the diethyl hypophosphite to 1-chloro-3-cyclopropane-2-propanol is 1:1.6; the mass of the catalyst 18-crown-6 is 5% of the mass of the diethyl hypophosphite.
[0067] Example 6
[0068] The disubstituted phosphinate compound has the structure shown in Formula I-2:
[0069]
[0070] The preparation method of the disubstituted phosphinate compound having the structure shown in formula I-2 comprises the following steps: adding 500 mL of toluene, 256 g of 1-chloro-3-cyclopropane-2-propanol, 217 g of diphenylphosphite and 10.8 g of tetrabutylammonium bromide into a reaction kettle, introducing nitrogen, heating to reflux state for substitution reaction for 20 h, cooling after the reaction is complete, adding water and ethyl acetate for extraction, combining the organic phases, drying, concentrating and spin drying to obtain 253 g of yellow solid, with a yield of 89%;
[0071] The molar ratio of the diphenyl phosphite to 1-chloro-3-cyclopropane-2-propanol is 1:1.6; the mass of the catalyst tetrabutylammonium bromide is 5% of the mass of the diphenyl phosphite.
[0072] Application Example 1
[0073] The preparation method of flame retardant epoxy resin cured product comprises the following steps:
[0074] Add 3 g of the disubstituted hypophosphite compound prepared in Example 1 to 10 g of epoxy resin (E51), mix well, add 9 g of methyltetrahydrophthalic anhydride and 0.2 g of triethylamine, mix and stir well, vacuum degas, pour into a test piece mold with a thickness of 3 mm, and finally place in an oven set at a temperature of 125° C. for curing for 1.5 h to obtain a clear and transparent flame-retardant epoxy resin cured product test piece;
[0075] The mass of the disubstituted phosphinate compound is 30% of the mass of the epoxy resin.
[0076] The flame retardant epoxy resin cured product specimen prepared in Application Example 1 was subjected to the UL94 vertical combustion test. The flame delay time was within 5 to 8 seconds twice, reaching the V0 grade. The softening point was about 85°C, and the hardness was >80D at room temperature.
[0077] Application Example 2
[0078] The preparation method of flame retardant epoxy resin cured product comprises the following steps:
[0079] Add 4 g of the disubstituted hypophosphite compound prepared in Example 1 to 10 g of epoxy resin (E51), mix well, add 9 g of methylhexahydrophthalic anhydride and 0.1 g of tris(dimethylaminomethyl)phenol, mix and stir well, vacuum degas, pour into a test piece mold with a thickness of 3 mm, and finally place in an oven set at a temperature of 145° C. for 2 h to obtain a clear and transparent flame-retardant epoxy resin cured product test piece;
[0080] The mass of the disubstituted phosphinate compound is 40% of the mass of the epoxy resin.
[0081] The flame retardant epoxy resin cured product specimen prepared in Application Example 2 was subjected to the UL94 vertical combustion test. The flame delay time was within 0 to 1 second for both tests, and the flame was basically extinguished as soon as it was removed from the flame, reaching the V0 grade. The softening point was about 100°C, and the hardness was >85D at room temperature.
[0082] Application Example 3
[0083] The preparation method of flame retardant epoxy resin cured product comprises the following steps:
[0084] Add 3.5 g of the disubstituted hypophosphite compound prepared in Example 1 to 10 g of epoxy resin (E51), mix well, add 9 g of methylhexahydrophthalic anhydride and 0.1 g of tris(dimethylaminomethyl)phenol, mix and stir well, vacuum degas, pour into a test piece mold with a thickness of 2 mm, and finally place in an oven set at a temperature of 145° C. for 2 h to obtain a clear and transparent flame-retardant epoxy resin cured product test piece;
[0085] The mass of the disubstituted phosphinate compound is 35% of the mass of the epoxy resin.
[0086] The flame retardant epoxy resin cured product test piece prepared in Application Example 3 was subjected to the UL94 vertical combustion test. The flame delay time was within 4-5 seconds twice, reaching the V0 grade. Its softening point was about 105°C, and its hardness was greater than 85D at room temperature.
[0087] Comparative Example 1
[0088] The preparation method of epoxy resin cured product comprises the following steps:
[0089] Add 4 g of dimethyl methyl phosphate (DMMP) to 10 g of epoxy resin (E51), mix well, add 9 g of methylhexahydrophthalic anhydride and 0.1 g of tris(dimethylaminomethyl)phenol, mix and stir well, vacuum degas, pour into a test piece mold with a thickness of 3 mm, and finally place in an oven set at a temperature of 145°C for curing for 2 hours to obtain an epoxy resin cured product test piece with uneven fog on the surface.
[0090] The epoxy resin cured product test piece prepared in Comparative Example 1 was subjected to the vertical combustion test of UL94. The test piece burned completely, and its softening point was about 65°C. The hardness was less than 85D at room temperature.
[0091] Comparative Example 2
[0092] The preparation method of epoxy resin cured product comprises the following steps:
[0093] Add 4 g of trichloroethyl phosphate (TCCP) to 10 g of epoxy resin (E51) and mix well; add 9 g of methylhexahydrophthalic anhydride and 0.1 g of tris(dimethylaminomethyl)phenol, mix and stir well, vacuum degas, pour into a test piece mold with a thickness of 3 mm, and finally place in an oven set at a temperature of 145°C for curing for 2 hours to obtain an epoxy resin cured product test piece with uneven fog on the surface.
[0094] The epoxy resin cured product test piece prepared in Comparative Example 2 was subjected to the vertical combustion test of UL94. The test piece burned completely, and its softening point was about 70°C. The hardness was less than 85D at room temperature.
[0095] In summary, the flame retardant epoxy resin cured product test pieces prepared in Application Examples 1 to 3 have significantly better flame retardant effects than those in Comparative Examples 1 to 2, and the flame retardant epoxy resin cured products prepared in Application Examples 1 to 3 are all clear and transparent with good physical properties. This indicates that the use of the disubstituted hypophosphite compound provided by the present invention as a flame retardant can prepare a transparent and clear flame retardant epoxy resin cured product with excellent flame retardant properties, achieve transparency of the flame retardant epoxy resin cured product, and reduce the adverse effects on the physical properties of the flame retardant foamed polyurethane material.
[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A disubstituted phosphinate compound, It is characterized in that It has the structure shown in formula I: In the formula I: 1 , R 2 , R 3 and R 4 are independently selected from hydrogen, C 1 ~C 8 The alkyl group, cycloalkyl group, aryl group or alkenyl group is selected from the group consisting of:
2. The method for preparing the disubstituted phosphinate compound according to claim 1, It is characterized in that The following steps are involved: A phosphinate having a structure of formula II, a halogenated compound having a structure of formula III, an organic solvent and a catalyst are mixed, and then a substitution reaction is carried out in an inert atmosphere to obtain a disubstituted phosphinate; In the formula II, R 1 and R 2 are independently selected from hydrogen, C 1 ~C 8 An alkyl, cycloalkyl, aryl or alkenyl group, M is a metal ion; In the formula III, R 3 and R 4 are independently selected from hydrogen, C 1 ~C 8 wherein the alkyl, cycloalkyl, aryl or alkenyl group is selected from the group consisting of:
3. The preparation method according to claim 2, It is characterized in that The organic solvent is one or more of toluene, xylene, dioxane, acetonitrile and tetrahydrofuran.
4. The preparation method according to claim 2, It is characterized in that The catalyst is at least one of a phase transfer catalyst and an amphoteric compound.
5. Use of the disubstituted phosphinate compound according to claim 1 or the disubstituted phosphinate compound prepared by the preparation method according to any one of claims 2 to 4 in preparing flame-retardant epoxy resin cured products.
6. The use according to claim 5, It is characterized in that The method for preparing the flame retardant epoxy resin cured product comprises the following steps: After the disubstituted phosphinate compound and the epoxy resin are mixed, an acid anhydride curing agent and a tertiary amine accelerator are added to perform curing to obtain a flame retardant epoxy resin cured product.
7. The use according to claim 6, It is characterized in that The mass of the disubstituted phosphinate compound is 7% to 45% of the mass of the epoxy resin.
8. The use according to claim 6, It is characterized in that The acid anhydride curing agent is at least one of methyltetrahydrophthalic anhydride and methylhexahydrophthalic anhydride.
9. The use according to claim 6, It is characterized in that The tertiary amine accelerator is at least one of triethylamine, triethylhydroxylamine, dimethylaminomethylphenol and tris(dimethylaminomethyl)phenol.
10. The use according to claim 6, It is characterized in that The curing temperature is 110° C. to 170° C., and the curing time is 1 to 4 hours.
Citation Information
Patent Citations
Flame retardant composite of epoxy resin and preparation method thereof
CN102875972A
Preparation method for hypophosphorous acid / phosphorous acid / phosphate compounds by adopting P(O)-OH-contained compounds
CN103980306A
Preparation method of dialkyl phosphinate
CN112661790A
Dialkyl phosphinate compound containing active epoxy group as well as preparation and application thereof
CN112778368A
Phosphorus-containing flame retardant mixture, method for producing said mixture and use of said mixture, and epoxy resin formulation comprising said flame retardant mixture
CN115916926A