Photocuring 3D printing high-toughness polyurethane resin and preparation method thereof
By preparing a combination of polyurethane prepolymer, diluent and photoinitiator, a high-strength and toughness photosensitive resin is formed, which solves the problem of insufficient strength and toughness of traditional orthopedic materials and realizes 3D printing materials with high mechanical properties and biocompatibility. , suitable for complex structures and personalized orthosis manufacturing.
Patent Information
- Application Number
- CN202410839823.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional orthopedic materials cannot have both high mechanical strength and high toughness, and cannot meet the needs of complex structures and personalized customization. Moreover, the existing high-strength photosensitive resin has poor toughness, resulting in poor impact resistance.
Using polyurethane prepolymer as the main raw material, through the combination with reactive diluent and free radical photoinitiator, a photo-cured 3D printing high-strength polyurethane resin with high strength and toughness is prepared. The synergistic effect of isocyanate and polyether is used to form a high-strength polyurethane resin. Cross-linked polymer network.
It achieves high tensile strength, elongation at break and bending strength of the material, has good mechanical properties and biocompatibility, is suitable for DLP and SLA 3D printers, and has low toxicity to cells, making it suitable for orthotics in the field of rehabilitation medicine. manufacture.
Smart Images

Figure CN118725211A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photocurable high-toughness polyurethane materials, and relates to a photocurable 3D printing high-strength and tough polyurethane resin suitable for orthotics and its preparation method. Background Art
[0002] With the development of rehabilitation engineering technology and the deepening of rehabilitation concepts, orthotics are being used more and more widely in rehabilitation technology, and the number of users is increasing year by year. Over the past 20 years, the manufacturing process of prostheses and orthotics has undergone significant changes. Traditional materials such as wood, metal, leather, and natural fiber fabrics are increasingly being replaced by modern polymer materials. This is mainly reflected in the application of thermoplastic sheets, resin-based composite materials, and low-temperature thermoplastic materials.
[0003] These new polymer materials enable a more scientific manufacturing process for prosthetic and orthotic products, better conforming to the requirements of human anatomy and biomechanics, and better meeting the demands for high strength, lightweight, corrosion resistance, and non-irritating properties for human products. However, most of these materials cannot simultaneously possess high mechanical strength and high toughness, and they often utilize traditional manufacturing processes, making them unsuitable for complex structures and personalized customization.
[0004] Currently available high-strength, glossy resins suitable for photopolymer 3D printing are mostly hard and brittle, with poor toughness. The difficulty in moving the spatial mesh also leads to high internal stress and poor impact resistance, resulting in brittle crack propagation when the product fails. High-toughness resins, on the other hand, struggle to balance material strength and cannot achieve corrective effects.
[0005] Therefore, there is an urgent need to develop a photosensitive resin that combines high strength and toughness to expand the application of 3D printing technology in the field of rehabilitation medicine. Summary of the Invention
[0006] To address the limitations of traditional orthodontic materials in simultaneously achieving high mechanical strength and high toughness, and thus failing to meet the demands of complex structures and personalized customization, this invention synthesizes a polyurethane prepolymer using inexpensive polyether raw materials. Furthermore, to overcome the technical deficiencies of existing technologies, this invention provides a photopolymerizable 3D printing high-strength and tough polyurethane resin and its preparation method.
[0007] In order to achieve the above-mentioned invention objectives, this application provides the following technical solutions:
[0008] First aspect:
[0009] A photopolymerizable 3D printing high-strength and tough polyurethane resin is composed of the following raw materials in weight percentages: 45-60% polyurethane prepolymer, 40-55% reactive diluent, and 1-3% free radical photoinitiator;
[0010] The polyurethane prepolymer has a molecular weight of 1000-5000, and the structural formula of the polyurethane prepolymer is:
[0011]
[0012] Where the number of n ranges from 20 to 40.
[0013] The structure of R1 includes One or more of them,
[0014] The structure of R2 includes One or more of them.
[0015] Preferably, the method for preparing the polyurethane prepolymer is as follows:
[0016] (1) Mix the polyether and isocyanate evenly, add the catalyst, and heat to the reaction temperature;
[0017] (2) Determine the isocyanate concentration and cool down the system after the concentration of isocyanate in the system no longer decreases.
[0018] (3) By adding the end-capping agent, polyurethane prepolymer can be obtained;
[0019] The raw materials for preparing the polyurethane prepolymer include, by mass percentage: 0.1-0.5 wt% catalyst, 0.1-1 wt% polymerization inhibitor, and the balance being polyether polyol, isocyanate, and hydroxyethyl acrylate; wherein the molar ratio of polyether polyol, isocyanate, and hydroxyethyl acrylate is 1:(2-3):(2-3).
[0020] Preferably, the raw materials for preparing the polyurethane prepolymer include, by mass percentage: 0.1 wt% catalyst, 0.3 wt% polymerization inhibitor, and the balance being polyether polyol, isocyanate and hydroxyethyl acrylate, wherein the molar ratio of polyether polyol, isocyanate and hydroxyethyl acrylate is 1:3:3.
[0021] Preferably, the raw materials for preparing the polyurethane prepolymer include, by mass percentage: 0.3 wt% catalyst, 0.2 wt% polymerization inhibitor, and the balance being polyether polyol, isocyanate and hydroxyethyl acrylate, wherein the molar ratio of polyether polyol to polyurethane is 1:3.
[0022] Preferably, the catalyst is one or more of dimethyltin dichloro, dibutyltin dilaurate mercaptan, dibutyltin dilaurate, dibutyltin diacetate, and dibutyltin maleate;
[0023] The isocyanate is one of isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), and hexamethylene diisocyanate (HDI);
[0024] The capping agent is one of hydroxyethyl acrylate (HEA), hydroxyethyl methacrylate (HEMA), and tert-butylaminoethyl methacrylate (TBAEMA);
[0025] The polymerization inhibitor is one or both of p-hydroxyanisole and hydroquinone.
[0026] Preferably, the reaction temperature in step (1) is controlled at 60-80°C and the reaction time is 2-4 hours; the reaction temperature in the second step is controlled at 45-50°C and the reaction time is 1-2 hours.
[0027] The temperature of the system described in step (2) is reduced to 45-50°C, preferably 50°C, and the reaction time is 1-2 hours.
[0028] Preferably, the free radical photoinitiator is (2,4,6-trimethylbenzoyl)diphenylphosphine oxide TPO-L, Irgacure LAP, or phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide XBPO.
[0029] Preferably, the reactive diluent is one or a combination of several of the following: hydroxyhexyl acrylate (HEA), N-vinylpyrrolidone (NVP), isobornyl acrylate (IBOA), isobornyl methacrylate (IBOMA), 2-phenoxyethyl acrylate (2-PEA), 3,3,5-trimethylcyclohexanol acrylate (TMCHA), tetrahydrofuran propylene (THFA), trimethylolpropane formal acrylate (CTFA), and acrylmorpholine (ACMO).
[0030] Preferably, the preparation method of the 3D printing photocurable high-strength and tough polyurethane resin includes the following steps:
[0031] 1) Preparation of polyurethane acrylate prepolymers with unsaturated double bonds;
[0032] 2) Weigh each raw material component that makes up the 3D printing photocurable elastic material according to the weight ratio; pre-disperse the free radical photoinitiator and the active diluent in a light-proof flat container, and then add the remaining material and stir to obtain a homogeneous liquid, which is the 3D printing photocurable resin material.
[0033] Preferably, the preparation method of the polyurethane acrylate prepolymer with unsaturated double bonds in step 1) includes the following steps:
[0034] 1.1) At room temperature, the polyether polyol and isocyanate were added to a four-necked round-bottom flask equipped with a mechanical stirrer, thermometer and dropping funnel, and stirred at 200 r / min;
[0035] 1.2) Add the catalyst slowly dropwise to the flask under a nitrogen atmosphere. After the catalyst is added, raise the temperature to 70°C and react for 2–4 hours.
[0036] 1.3) The NCO group composition of the reactants was continuously monitored using Fourier transform infrared spectroscopy (FT-IR);
[0037] 1.4) When the absorption peak of the NCO group stops decreasing, the reaction temperature is lowered to 50℃ and the end-capping agent HEA is added dropwise to the reactants to continue the reaction for 1-2 hours;
[0038] 1.5) After the NCO absorption peak disappears, add 0.1% of the polymerization inhibitor MEHQ to prevent the polymerization of double bonds in the oligomer to obtain a transparent, viscous liquid PUA oligomer.
[0039] The second aspect:
[0040] A photocurable polyurethane prepolymer was prepared by end-capping with polyether and isocyanate as the soft and hard segments in the molecular structure, respectively. The synthesis process is shown below:
[0041]
[0042] (1) Compared with the prior art, this invention, based on this oligomer, obtains a photosensitive resin with both high strength and toughness by combining it with a series of biosafe diluents. Due to the highly cross-linked polymer network and the synergistic effect of the rigidity of the isocyanate and the flexibility of the long polyether chains, the 3D printing material exhibits the expected mechanical properties, with a tensile strength exceeding 40 MPa, an elongation at break greater than 100%, a flexural strength of over 33 MPa, and a flexural modulus of over 1000 MPa. This photosensitive resin is suitable for DLP and SLA 3D printers and can print samples under both 365 nm and 405 nm ultraviolet light. The photocurable material exhibits low cytotoxicity to (L929) cells and no skin irritation to animals.
[0043] (2) The orthotics designed and successfully printed by this invention exhibit high printing precision and possess advantages similar to low-temperature thermoplastic sheets, such as being non-toxic, non-irritating, lightweight, having good shape memory, being easy to shape, breathable, lightweight, and comfortable. Its overall mechanical properties far exceed those of low-temperature thermoplastic sheets. The material's excellent mechanical properties and biocompatibility will provide more options for developing customized orthotics materials, while simultaneously improving wearing comfort and extending its service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0045] Figure 1 It is a polyether raw material 1 H NMR spectrum;
[0046] Figure 2 It is the polyurethane prepolymer prepared. 1 H NMR spectrum;
[0047] Figure 3 These are the infrared spectra of the raw materials and the synthesized prepolymer;
[0048] Figure 4 The image shows the GPC characterization spectrum of the prepared prepolymer.
[0049] Figure 5 These are the tensile and bending strain curves of the 3D printed sample.
[0050] Figure 6 These are the thermogravimetric and DMA curves of the 3D printed sample.
[0051] Figure 7 These are cell activity graphs from different extracts;
[0052] Figure 8 This is a schematic diagram of cell fluorescence staining;
[0053] Figure 9 This is a schematic diagram of an orthopedic device printed using SLA and DLP printers. Detailed Implementation
[0054] The present application is further illustrated below with reference to specific embodiments. The following descriptions are merely a few embodiments of the present application and are not intended to limit the present application in any way. Although the present application discloses preferred embodiments as follows, they are not intended to limit the present application. Any modifications or variations made by those skilled in the art without departing from the scope of the technical solution of the present application using the disclosed technical content are equivalent to equivalent implementation cases and all fall within the scope of the technical solution.
[0055] Unless otherwise specified, the raw materials used in the embodiments of this application are all purchased commercially and used directly without any special treatment.
[0056] Unless otherwise specified, the analytical methods in the embodiments all adopt conventional instrument or equipment settings and conventional analytical methods.
[0057] The raw materials in the following examples are derived from…
[0058] Mechanical property testing: The prepared acrylate prepolymer was mixed with an reactive diluent to form a light-curing resin, which was then cured into dumbbell-shaped specimens using an SLA and DLP light engine. The mechanical properties of the specimens were tested using a universal testing machine (UT-2080) according to GB / T 528-2009. The clamp spacing was 25 mm, the specimen width was 5 mm, the thickness was 2 ± 0.2 mm, and the tensile rate was 10 mm / min. The flexural strength and flexural modulus of the material were tested according to GB / T9341-2008, with a specimen width of 10 mm, a thickness of 4 mm, a span of 64 mm, and a bending rate of 5 mm / min.
[0059] Example 1
[0060] At room temperature, 333 g of isophorone diisocyanate (IPDI), 0.83 g of catalyst (DBTDL), and 50 ml of solvent cyclohexane were added to a four-necked round-bottom flask equipped with a mechanical stirrer, thermometer, and dropping funnel. Then, under nitrogen protection, 500 g of pentaerythritol polyether polyol (Mn = 1000) was slowly added dropwise to the flask while stirring at 200 rpm. After the addition was complete, the temperature was raised to 70 °C, and the reaction was stirred for 2 hours. The NCO group composition of the reactants was continuously monitored using Fourier transform infrared spectroscopy (FT-IR). When 2266 cm⁻¹... -1 When the absorption peak intensity of the NCO group stopped decreasing, the reaction temperature was lowered to 50℃, and 174g of end-capping agent HEA was added dropwise to the reactants. After reacting for 1 hour, the NCO absorption peak was detected using FT-IR. After the NCO absorption peak disappeared, 1g of polymerization inhibitor MEHQ was added to prevent the polymerization of double bonds in the oligomer, and the solvent was removed using a rotary evaporator at 40℃ to obtain a transparent, viscous liquid PUA oligomer. The polyether polyol raw material (…) was analyzed by 1H NMR spectroscopy. Figure 1 ) and products ( Figure 2 Characterization revealed that the chemical shift of the methyl group in the polyether segment was 1.1 ppm, and the peak at 7.9 ppm was attributed to -NH. Furthermore, the peaks at 5.8 ppm, 6.2 ppm, and 6.5 ppm were attributed to the -CH=CH2 groups of the acrylate. This indicates that the isocyanate group and double bond have been successfully incorporated into the polyether molecular structure.
[0061] Example 2
[0062] Compared with Example 1, the only difference is the change in the molecular weight of the polyether polyol; all other conditions are the same as in Example 1. The specific operation is as follows:
[0063] At room temperature, 500 g of polyether polyol (Mn = 3000) and 0.61 g of DBTDL were added to a four-necked round-bottom flask equipped with a mechanical stirrer, thermometer, and dropping funnel. Then, under a nitrogen atmosphere, 111 g of IPDI was slowly added dropwise while stirring at 200 rpm. After the addition of IPDI, the temperature was raised to 70°C, and the reaction was stirred for 2 hours. The isocyanate groups in the system were titrated according to standard HG / T2409-92. When the amount of NCO groups stopped decreasing, the reaction temperature was lowered to 50°C, and 56 g of end-capping agent HEA and 0.1% polymerization inhibitor MEHQ were added dropwise to the reactants to prevent double bond polymerization in the oligomers. After 1 hour of reaction, the NCO absorption peak was detected using FT-IR. After the NCO absorption peak disappeared, the reaction was stopped, and the product was degassed under vacuum to obtain a transparent, viscous liquid PUA oligomer.
[0064] GPC test results are as follows Figure 4 As shown, the number-average molar mass (Mn) and weight-average molar mass (Mw) of PUA-3000 oligomers are 3831 kg / mol and 4099 kg / mol, respectively. The (Mw / Mn) values are 1.03 and 1.07, respectively, indicating that no polymerization occurred during the reaction, and the molecular weight distribution is relatively narrow.
[0065] Example 3
[0066] The method is the same as in Example 1, except that the functionality and molecular weight of the polyether are different. All other conditions are the same as in Example 1. The specific operation is as follows:
[0067] At room temperature, 111 g of isophorone diisocyanate (IPDI) and 0.61 g of DBTDL were added to a four-necked round-bottom flask equipped with a mechanical stirrer, thermometer, and dropping funnel. Then, polyether (Mn = 2000) was slowly added dropwise to the flask under a nitrogen atmosphere while stirring at 200 rpm. After the addition, the temperature was raised to 70°C and the reaction was stirred for 2 hours. The isocyanate groups in the system were titrated according to standard HG / T2409-92. When the amount of NCO groups stopped decreasing, the reaction temperature was lowered to 50°C, and 58 g of end-capping agent HEA and 0.7 g of polymerization inhibitor MEHQ were added dropwise to the reactants to prevent double bond polymerization in the oligomers. After 1 hour of reaction, the NCO absorption peak was detected using FT-IR. After the NCO absorption peak disappeared, the reaction was stopped, and the product was degassed under vacuum to obtain a transparent, viscous liquid PUA oligomer. The obtained product was characterized by infrared spectroscopy. Figure 3 ), in the spectrum at 1107 cm⁻¹ -1 There is a characteristic peak of COC at 1727 cm⁻¹. -1 The absorption peak is for C=O, representing a characteristic peak of the ester group. At 1638 cm⁻¹ -1The C=C stretching vibration peak appearing at 2266 cm⁻¹ also confirms the successful introduction of the acrylate group. Furthermore, the peak at 2266 cm⁻¹... -1 The absence of characteristic peaks for NCO groups indicates that -NCO and HEA have completely reacted.
[0068] Product Example 4
[0069] A photopolymerizable 3D printing high-strength and tough polyurethane resin material comprises the following raw materials by weight percentage: 50% prepolymer, 15% hydroxyethyl methacrylate, 33% N-vinylpyrrolidone, 1.5% free radical photoinitiator, 0.2% fluorescent whitening agent, and 0.3% antioxidant.
[0070] The prepolymer is the polyurethane PUA prepared in Example 1.
[0071] The free radical photoinitiator is Irgacure 819.
[0072] The fluorescent whitening agent is KCB.
[0073] The antioxidant is 1010.
[0074] Weigh the raw materials according to the weight ratio, pre-disperse the solid free radical photoinitiator powder and the reactive diluent in the dark for 15 minutes, then add the other raw materials and stir them together at 60°C to obtain a homogeneous liquid.
[0075] Product Example 5
[0076] Compared with Product Example 4, the only difference is the component ratio; all other conditions are the same as in Product Example 4. The specific operation is as follows:
[0077] A photopolymerizable 3D printing high-strength and tough polyurethane resin material comprises the following raw materials by weight percentage: 55% prepolymer, 42% acryloylmorpholine, 2.5% free radical photoinitiator, and 0.5% additives.
[0078] The prepolymer is a mixture of the polyurethane prepared in Example 1 and the polyurethane prepared in Example 2 in a mass ratio of 3:1.
[0079] The free radical photoinitiator is TPO-L.
[0080] The adjuvant is antioxidant 168.
[0081] Weigh the raw materials according to the weight ratio, pre-disperse the solid free radical photoinitiator powder and the reactive diluent in the dark for 15 minutes, then add the other raw materials and stir them together at 60°C to obtain a homogeneous liquid.
[0082] Product Example 6
[0083] A formulation for a high-strength, high-toughness polyurethane resin for photocurable 3D printing: 45 wt% reactive diluent and 2 wt% TPO-L were simultaneously added to a brown, light-proof medium, and the mixture was magnetically stirred for 15 min. Then, 53 wt% of the product from Example 3 was added, and stirring continued for 30 min. The mixture was then ultrasonically degassed to obtain the photocurable resin. The obtained photocurable resin was cured using a DLP photocuring engine, and the mechanical properties of the cured samples were measured.
[0084] Table 1. Test results of material mechanical properties
[0085]
[0086] To assess mechanical strength and toughness, the material's mechanical properties were measured, and the results are as follows: Figure 5 As shown in Table 1, the polyurethane material provided by this invention possesses excellent toughness, tensile properties, and fatigue resistance. Its unique skeletal structure with alternating HS and SS segments and microphase separation enhances the mechanical properties of the photopolymer, including high strength and excellent tensile strength. The resin components form an interpenetrating network during photocuring, giving it both strength and toughness.
[0087] like Figure 6 Thermal performance results show that it does not soften or deform over a wide temperature range. Biocompatibility testing is a key step in assessing the toxicity of materials in biomedical applications, and good biocompatibility is also an essential condition for wearable devices.
[0088] like Figure 7 As shown, the samples were extracted with the widely used DEME high-glucose medium and the highly soluble DMSO, respectively. The results showed that even with a high concentration of 10 mg / mL extract, the cell viability was still higher than 80%.
[0089] Depend on Figure 8 As shown, most cells survived in the high-concentration sample and showed a similar proliferation trend compared to the control group.
[0090] like Figure 9 As shown, the resin has a fine 3D structure and can be used to manufacture orthopedic models for medical devices using both SLA and DLP technologies. Based on the high strength and biocompatibility of this 3D printing material, its potential applications in the medical field can be foreseen.
[0091] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A photocurable 3D printing high-toughness polyurethane resin, characterized in that: The method is composed of the following raw materials in percentage by mass: 45-60% of polyurethane prepolymer, 40-55% of active diluent, and 1-3% of free radical photoinitiator; The molecular weight of the polyurethane prepolymer is 1000-5000, and the structural formula of the polyurethane prepolymer is: Among them, the number of n is 20 to 40, The structure of R1 includes One or more of which, the structure of R2 includes One or more of these.
2. The 3D printing light-curable high-toughness polyurethane resin according to claim 1, characterized in that: The preparation method of the polyurethane prepolymer is: (1) mixing polyether and isocyanate uniformly, adding a catalyst, and heating to a reaction temperature; (2) measuring the isocyanate content, waiting until the concentration no longer decreases, and lowering the temperature; (3) adding a capping agent dropwise to obtain a polyurethane prepolymer; The raw materials for preparing the polyurethane prepolymer include, by mass percentage, 0.1-0.5wt% of a catalyst, 0.1-1wt% of a polymerization inhibitor, and the remainder being polyether polyol, isocyanic acid, and hydroxyethyl acrylate; wherein the molar ratio of the polyether polyol, isocyanic acid, and hydroxyethyl acrylate is 1:(2-3):(2-3).
3. The 3D printing light-curable high-toughness polyurethane resin according to claim 2, characterized in that: The raw materials for preparing the polyurethane prepolymer include, by mass percentage, 0.1wt% of a catalyst, 0.3wt% of a polymerization inhibitor, and the remainder of polyether polyol, isocyanic acid and hydroxyethyl acrylate, wherein the molar ratio of polyether polyol, isocyanic acid and hydroxyethyl acrylate is 1:3:
3.
4. A 3D printing light-cured high-toughness polyurethane resin as claimed in claim 3, characterized in that: The raw materials for preparing the polyurethane prepolymer include, by mass percentage, 0.3wt% of a catalyst, 0.2wt% of a polymerization inhibitor, and the remainder of polyether polyol, isocyanic acid and hydroxyethyl acrylate, wherein the molar ratio of polyether polyol to polyurethane is 1:
3.
5. The 3D printing light-curable high-toughness polyurethane resin according to any one of claims 2 to 4, characterized in that: The catalyst is one or more of dimethyltin dichloride, dibutyltin dilaurate mercaptan, dibutyltin dilaurate, dibutyltin diacetate, and dibutyltin maleate; The isocyanic acid is one of isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), and hexamethylene diisocyanate (HDI); The end-capping agent is one of hydroxyethyl acrylate (HEA), hydroxyethyl methacrylate (HEMA), and tert-butylaminoethyl methacrylate (TBAEMA); The polymerization inhibitor is one or both of p-hydroxyanisole and hydroquinone.
6. A 3D printing light-cured high-toughness polyurethane resin as claimed in claim 2, characterized in that: The reaction temperature in step (1) is controlled at 60-80° C. and the reaction time is 2-4 h; In step (2), the temperature of the system is reduced to 45-50° C., preferably 50° C., and the reaction time is 1-2 h.
7. A 3D printing light-curable high-toughness polyurethane resin as claimed in claim 1, characterized in that: The free radical photoinitiator is (2,4,6-trimethylbenzoyl) diphenylphosphine oxide TPO-L, Irgacure LAP or phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide XBPO.
8. A 3D printing light-curable high-toughness polyurethane resin as claimed in claim 1, characterized in that: The active diluent is one or a combination of 2-hydroxyhexyl acrylate HEA, N-vinyl pyrrolidone NVP, isobornyl acrylate IBOA, isobornyl methacrylate IBOMA, 2-phenoxyethyl acrylate 2-PEA, 3,3,5-trimethylcyclohexanol acrylate TMCHA, tetrahydrofuran propylene THFA, trimethylolpropane formal acrylate CTFA and acryloyl morpholine ACMO.
9. A method for preparing the 3D printing light-cured high-toughness polyurethane resin according to claim 2, characterized in that The steps include: 1) preparing a polyurethane acrylate prepolymer having an unsaturated double bond; 2) Weighing the raw material components constituting the 3D printing light-curing elastic material according to the weight ratio; pre-dispersing the free radical photoinitiator and the active diluent in a light-proof plane at the same time, and then adding the remaining materials and stirring to obtain a homogeneous liquid, which is the 3D printing light-curing resin material.
10. A method for preparing the 3D printing light-curable high-toughness polyurethane resin according to claim 9, characterized in that: The preparation method of the polyurethane acrylate prepolymer having unsaturated double bonds described in step 1) comprises the following steps: 1.1) Add polyether polyol and isocyanate into a four-necked round-bottom flask equipped with a mechanical stirrer, a thermometer and a dropping funnel at room temperature and stir at 200 r / min; 1.2) Slowly drop the catalyst into the flask under nitrogen atmosphere. After the dropwise addition, the temperature rises to 70°C and the reaction is continued for 2 to 4 hours. 1.3) Continuously monitor the NCO group composition of the reactants using Fourier transform infrared spectroscopy (FT-IR); 1.4) When the absorption peak of the NCO group stops decreasing, the reaction temperature is reduced to 50°C, and the end-capping agent HEA is added dropwise to the reactants to continue the reaction for 1 to 2 hours; 1.5) After the NCO absorption peak disappears, 0.1% of inhibitor MEHQ is added to prevent the double bond polymerization in the oligomer to obtain a transparent viscous liquid PUA oligomer.
Citation Information
Patent Citations
Polyurethane acrylate oligomer and preparation method thereof
CN102911337A
Hydrogel, which is formed by in situ radiation curing of at least one urethane acrylate-precursor, useful for treating wounds, where the precursor is obtained from polyalkylene oxide, diisocyanate and unsaturated alcohol
DE102008023798A1
Resin composition for 3D printer, method for producing same, and cured product
US20240084066A1
Cited By
Shape memory polymer-based 4D printed invisible orthodontic appliance material, preparation method and application thereof, and 4D printed invisible orthodontic appliance
CN119390904A
4D printing aligner material based on shape memory polymer and preparation method and application thereof, and 4D printing aligner
CN119390904B
Light-cured polyurethane composition for 3D printing and use method of light-cured polyurethane composition
CN121975078A