Preparation method of nitrogen-phosphorus flame-retardant modified polyurethane porous foam material

A nitrogen-phosphorus cyclic polyol is generated by reacting hexachlorocyclotriphosphazene with triethanolamine. This polyol is then used to prepare nitrogen-phosphorus flame-retardant modified polyurethane porous foam materials, which solves the problem of flammability of polyurethane porous foam and achieves high-efficiency flame retardancy and low density.

CN118725232APending Publication Date: 2024-10-01ZHEJIANG UNIV OF TECH TONGXIANG RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410842985.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Polyurethane porous foam materials are flammable, burn rapidly, and produce toxic gases. Existing flame retardant methods suffer from poor compatibility and reduced flame retardant performance.

Method used

A nitrogen-phosphorus flame-retardant modified polyurethane porous foam material was prepared by reacting hexachlorocyclotriphosphazene with triethanolamine to generate a polyol containing a nitrogen-phosphorus cyclic structure, and then reacting it with isocyanate to produce a polyurethane foam.

Benefits of technology

It achieves excellent flame retardancy and low density, improving the safety and mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of flame-retardant materials, and discloses a preparation method of a nitrogen-phosphorus flame-retardant modified polyurethane porous foam material. According to the preparation method disclosed by the invention, hexachlorocyclotriphosphazene reacts with triethanolamine to obtain polyhydric alcohol containing a nitrogen-phosphorus cyclic structure. Then, the modified polyol and isocyanate are subjected to a polyurethane foaming reaction, and the finally obtained nitrogen-phosphorus flame-retardant modified polyurethane porous foam material has excellent flame retardance and relatively low density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of flame retardant materials, in particular to a method for preparing a nitrogen-phosphorus flame retardant modified polyurethane porous foam material. Background Art

[0002] Polyurethane foam is a polymer material made of isocyanate and polyester or polyether polyols in the presence of a variety of additives such as foaming agents, catalysts, and surfactants. Polyurethane porous foam has excellent thermal insulation properties, high compressive strength, and a simple production process, and is widely used in sofa furniture, clothing, automobiles, and other fields. However, polyurethane porous foam itself is extremely flammable, has a low limiting oxygen index and a fast burning speed, and also produces high-temperature droplets and toxic gases during the combustion process, greatly increasing the risk during use. In order to meet people's demand for safety, polyurethane porous foam must be flame-retardant treated.

[0003] At present, there are two methods for flame retardant treatment of polyurethane foam. One is to use an additive flame retardant. By adding the additive flame retardant before polyurethane foaming, polyurethane foam with flame retardant effect can be foamed. This method has low cost and simple process, but it also has disadvantages such as poor compatibility with the matrix, affecting the mechanical properties of the foam, easy migration of the flame retardant, and the flame retardant property will weaken over time. Another method is to introduce a functional monomer with flame retardant properties into a long chain segment of polyurethane by chemical grafting, thereby obtaining a flame retardant effect. The present invention applies the second method, introduces flame retardant functional groups into polyols and then foams to obtain porous polyurethane foam with flame retardant effect. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a nitrogen-phosphorus flame-retardant modified polyurethane porous foam material. The present invention utilizes hexachlorocyclotriphosphazene to react with triethanolamine to obtain a polyol containing a nitrogen-phosphorus ring structure. The modified polyol is then subjected to a polyurethane foaming reaction with isocyanate, and the resulting nitrogen-phosphorus flame-retardant modified polyurethane porous foam material has excellent flame retardancy and low density.

[0005] The specific technical scheme of the present invention is: a method for preparing a nitrogen-phosphorus flame-retardant modified polyurethane porous foam material, comprising the following steps:

[0006] 1) adding hexachlorocyclotriphosphazene to an organic solvent, heating to reflux, stirring and mixing evenly, and then dropping triethanolamine to react; the molar ratio of triethanolamine to hexachlorocyclotriphosphazene is 2.5-3.5:1.

[0007] In step 1), the present invention utilizes six chlorine atoms in hexachlorocyclotriphosphazene to react with two hydroxyl groups in three triethanolamines to obtain a polyol containing a nitrogen-phosphorus ring structure.

[0008] 2) cooling, adding sodium bicarbonate solution to the reaction product of step 1) to react; the molar ratio of the sodium bicarbonate to the hexachlorocyclotriphosphazene is 5-7:1.

[0009] The addition of sodium bicarbonate solution in this step is mainly to neutralize the acid produced in the reaction in step 1) and promote the substitution reaction to move forward. Too little addition will lead to incomplete reaction and low yield, thus affecting the subsequent flame retardant effect.

[0010] 3) After the reaction is completed, dimethylformamide solvent is added to the reaction product of step 2), and the mixture is heated and stirred; after standing, an equal amount of deionized water is added, and after a granular salt product precipitates at the bottom of the container, the upper layer solution is separated.

[0011] The target product is easily soluble in dimethylformamide solvent, while other impurities have low solubility in dimethylformamide and will produce precipitation after adding water. Therefore, the above method is used to separate and purify the target product for subsequent reaction.

[0012] 4) The upper solution, polyethylene glycol and catalyst are added to the reactor, and the reaction is heated at 110-130°C for 2-3 hours under vacuum and stirring conditions, and then the temperature is lowered to 65-75°C, and chain extender A and chain extender B, internal crosslinking agent trimethylolpropane and solvent are added, and the reaction is continued for 1.5-2.5 hours.

[0013] The present invention divides step 4) into two stages. First, the reactor is vacuumed and heated to 110-130° C. to remove moisture from the raw materials. Then, a chain extender and an internal crosslinking agent are added to avoid gelation of the polyurethane during the subsequent reaction.

[0014] The molar ratio of the polyethylene glycol to the hexachlorocyclotriphosphazene is (0.8-1.2):1; the amounts of the chain extender A, chain extender B and internal crosslinking agent are 8-9%, 3-3.5% and 1.5-1.7% (more preferably 9%, 3.5% and 1.6%) of the mass of the reaction system respectively.

[0015] The role of adding chain extenders and cross-linking agents is to form molecular chains by reacting with isocyanates, causing polyurethane to undergo cross-linking, thereby improving its mechanical properties, wear resistance, and corrosion resistance. However, the addition of too much chain extender and cross-linking agent will consume more isocyanate, making the resulting polyurethane foam hard and brittle, affecting its mechanical properties.

[0016] 5) After the reaction is completed, the system is cooled to room temperature, glacial acetic acid is added for neutralization, the product is taken out, water is added, hexamethylene diisocyanate, catalyst tetramethylethylenediamine and foaming agent azodicarbonamide are added, and after stirring evenly, the mixture is poured into a mold and allowed to stand for foaming.

[0017] 6) After the foaming is completed, the polyurethane porous foam material is heated and aged to obtain a nitrogen-phosphorus flame-retardant modified polyurethane foam material.

[0018] In summary, the nitrogen-phosphorus flame-retardant modified polyurethane porous foam material finally obtained by the method of the present invention has excellent flame retardancy and low density.

[0019] Preferably, in step 1), the reaction temperature is 130-150° C., and the reaction time is 1-3 h.

[0020] Preferably, in step 1), the organic solvent is selected from one or more of acetone, toluene, xylene and tetrahydrofuran.

[0021] Preferably, in step 2), the temperature after cooling is 80-90° C.; and the reaction time is 1.5-2 h.

[0022] Preferably, in step 3), the mass ratio of the amount of the dimethylformamide solvent to the amount of the hexachlorocyclotriphosphazene is 5-7:1.

[0023] Preferably, in step 3), the heating and stirring is performed at a temperature of 40-50° C. and for a time of 0.5-1.5 h.

[0024] Preferably, in step 4), the catalyst is dibutyltin dilaurate; the chain extender A is N-methyldiethanolamine; the chain extender B is 1,4-butanediol; and the solvent is N-methylpyrrolidone.

[0025] Preferably, in step 4), the pressure of the reactor is 0.08-0.12 MPa.

[0026] Preferably, in step 5), the amount of glacial acetic acid added is 3-6wt% of the reaction system; the neutralization time is 20-40min; the amount of water added is 2-4wt% of the polyethylene glycol; the molar ratio of hexamethylene diisocyanate to hexachlorocyclotriphosphazene is 1:4-6. The amount of the catalyst tetramethylethylenediamine used is 0.1-0.2% of the mass of the reaction system, and the amount of the blowing agent azodicarbonamide used is 0.1-0.3% of the mass of the reaction system.

[0027] Preferably, in step 5), the stirring time is 5-15s; the mold is preheated at 35-45°C; and the foaming is completed when the foam expands and solidifies in the mold.

[0028] Preferably, in step 6), the aging temperature is 70-90° C. and the time is 20-30 hours.

[0029] Compared with the prior art, the invention has the following beneficial effects: the invention uses hexachlorocyclotriphosphazene to react with triethanolamine to obtain a polyol containing a nitrogen-phosphorus ring structure. The modified polyol is then subjected to a polyurethane foaming reaction with isocyanate, and the nitrogen-phosphorus flame-retardant modified polyurethane porous foam material finally obtained has excellent flame retardancy and a relatively low density. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with the embodiments.

[0031] Example 1

[0032] (1) Weigh 34.7 g of hexachlorocyclotriphosphazene and dissolve it in 150 mL of toluene in a three-necked flask. Fix the three-necked flask in a constant temperature oil bath, install a condenser at one end, set the temperature to 120° C., so that the toluene refluxes, and start stirring to fully mix the materials.

[0033] (2) Weigh 44.8 g of triethanolamine and dissolve it in 50 mL of toluene. Add the mixture dropwise into a three-necked flask using a constant pressure dropping funnel and allow to react for 2 hours.

[0034] (3) After the reaction is completed, the temperature of the oil bath is adjusted to 85°C, 50.4 g of sodium bicarbonate is weighed and dissolved in deionized water, and the sodium bicarbonate solution is added to the system to generate a large number of bubbles. The reaction is continued for another 2 hours until no bubbles are generated during the reaction, indicating that the reaction is complete.

[0035] (4) After the reaction, adjust the temperature of the oil bath to 45°C, add an appropriate amount of dimethylformamide solvent to the product, stir thoroughly, and then let it stand for 1 hour.

[0036] (5) After standing for a period of time, granular salt product precipitates appear at the bottom of the bottle, and the upper liquid is separated for later use.

[0037] (6) Weigh 30 g of polyethylene glycol 300 and the separated upper liquid and add them to a jacketed reactor with a stirrer, and then add 1 ml of dibutyltin dilaurate. Pour an appropriate amount of heat transfer oil into the high-temperature circulator, connect the reactor, turn on the heating cycle of the high-temperature circulator, and set the temperature to 120°C. Then connect the jacketed reactor to a vacuum pump, turn on the vacuum pump, make the system pressure at 0.1 MPa, turn on the stirrer, accelerate the mixing of the materials, and evacuate for 2.5 hours.

[0038] (7) Without turning off the agitator and vacuum pump, adjust the temperature of the high-temperature circulator to 70°C, weigh 9.4 g of N-methyldiethanolamine, 3.5 g of 1,4-butanediol, and 1.8 g of trimethylolpropane. When the temperature of the reactor drops to 70°C, add the weighed chemicals into the reactor and continue the reaction for 2 hours.

[0039] (8) After the reaction is completed, the system is cooled to room temperature, and then 3.5 g of glacial acetic acid is added to neutralize for 30 min. Then, the product obtained in the reactor is taken out and added to a round-bottom flask, and then 2.4 g of water is added. Stirring is started at a speed of 1500 r / min to ensure that the materials are fully mixed.

[0040] (9) Weigh 42.0 g of hexamethylene diisocyanate, and then weigh 0.2 g of tetramethylethylenediamine (catalyst) and 0.2 g of azodicarbonamide (foaming agent) and quickly add them into a round-bottom flask. Adjust the stirring speed of the stirrer to 3000 r / min. After 10 seconds, pour the mixed solution in the round-bottom flask into a mold that has been preheated to 40°C.

[0041] (10) The foam was allowed to stand in the mold for 30 min, and then the cured foam was placed in an oven at 80 °C to complete a 24 h curing process.

[0042] Example 2

[0043] (1) Weigh 52.1 g of hexachlorocyclotriphosphazene and dissolve it in 170 mL of toluene in a three-necked flask. Fix the three-necked flask in a constant temperature oil bath, install a condenser at one end, set the temperature to 120° C., so that the toluene refluxes, and start stirring to fully mix the materials.

[0044] (2) Weigh 67.1 g of triethanolamine and dissolve it in 70 mL of toluene. Add the mixture dropwise into a three-necked flask using a constant pressure dropping funnel and allow to react for 2 hours.

[0045] (3) After the reaction is completed, the temperature of the oil bath is adjusted to 85°C, 75.6 g of sodium bicarbonate is weighed and dissolved in deionized water, and the sodium bicarbonate solution is added to the system. A large number of bubbles are generated by the reaction, and the reaction is continued for 1.5-2 hours. When the reaction stops generating bubbles, the reaction is completed.

[0046] (4) After the reaction, adjust the temperature of the oil bath to 45°C, add an appropriate amount of dimethylformamide solvent to the product, stir thoroughly, and then let it stand for 1 hour.

[0047] (5) After standing for a period of time, granular salt product precipitates appear at the bottom of the bottle, and the upper liquid is separated for later use.

[0048] (6) Weigh 45g of polyethylene glycol 300 and the separated upper liquid and add them to a jacketed reactor with a stirrer, and then add 1ml of dibutyltin dilaurate. Pour an appropriate amount of heat transfer oil into the high-temperature circulator, connect the reactor, turn on the heating cycle of the high-temperature circulator, and set the temperature to 120°C. Then connect the jacketed reactor to a vacuum pump, turn on the vacuum pump, make the system pressure at 0.1MPa, turn on the stirrer, accelerate the mixing of the materials, and evacuate for 2.5 hours.

[0049] (7) Without turning off the agitator and vacuum pump, adjust the temperature of the high-temperature circulator to 70°C, weigh 18.2 g of N-methyldiethanolamine, 6.8 g of 1,4-butanediol, and 3.4 g of trimethylolpropane. When the temperature of the reactor drops to 70°C, add the weighed chemicals into the reactor and continue the reaction for 2 hours.

[0050] (8) After the reaction is completed, the system is cooled to room temperature, and then 6.8 g of glacial acetic acid is added to neutralize for 30 min. Then, the product obtained in the reactor is taken out and added to a round-bottom flask, and then 4.5 g of water is added. Stirring is started at a speed of 1500 r / min to ensure that the materials are fully mixed.

[0051] (9) Weigh 63.1 g of hexamethylene diisocyanate, 0.3 g of tetramethylethylenediamine (catalyst), and 0.4 g of azodicarbonamide (foaming agent) and quickly add them into a round-bottom flask. Adjust the stirring speed of the stirrer to 3000 r / min. After 10 seconds, pour the mixed solution in the round-bottom flask into a mold that has been preheated to 40°C.

[0052] (10) The foam was allowed to stand in the mold for 30 min, and then the cured foam was placed in an oven at 80 °C to complete a 24 h curing process.

[0053] Example 3

[0054] (1) Weigh 69.5 g of hexachlorocyclotriphosphazene and dissolve it in 180 mL of toluene in a three-necked flask. Fix the three-necked flask in a constant temperature oil bath, install a condenser at one end, set the temperature to 120° C., so that the toluene refluxes, and start stirring to fully mix the materials.

[0055] (2) Weigh 89.5 g of triethanolamine and dissolve it in 100 mL of toluene. Add the mixture dropwise into a three-necked flask using a constant pressure dropping funnel and allow to react for 2 hours.

[0056] (3) After the reaction is completed, the temperature of the oil bath is adjusted to 85°C, 100.8 g of sodium bicarbonate is weighed and dissolved in deionized water, and the sodium bicarbonate solution is added to the system to generate a large number of bubbles. The reaction is continued for 1.5-2 hours. When no bubbles are generated during the reaction, the reaction is completed.

[0057] (4) After the reaction, adjust the temperature of the oil bath to 45°C, add an appropriate amount of dimethylformamide solvent to the product, stir thoroughly, and then let it stand for 1 hour.

[0058] (5) After standing for a period of time, granular salt product precipitates appear at the bottom of the bottle, and the upper liquid is separated for later use.

[0059] (6) Weigh 60g of polyethylene glycol 300 and the separated upper liquid and add them to a jacketed reactor with a stirrer, and then add 1ml of dibutyltin dilaurate. Pour an appropriate amount of heat transfer oil into the high-temperature circulator, connect the reactor, turn on the heating cycle of the high-temperature circulator, and set the temperature to 120°C. Then connect the jacketed reactor to a vacuum pump, turn on the vacuum pump, make the system pressure at 0.1MPa, turn on the stirrer, accelerate the mixing of the materials, and evacuate for 2.5 hours.

[0060] (7) Without turning off the agitator and vacuum pump, adjust the temperature of the high-temperature circulator to 70°C, weigh 24.2 g of N-methyldiethanolamine, 9.1 g of 1,4-butanediol, and 4.5 g of trimethylolpropane. When the temperature of the reactor drops to 70°C, add the weighed chemicals into the reactor and continue the reaction for 2 hours.

[0061] (8) After the reaction is completed, the system is cooled to room temperature, and then 9.1 g of glacial acetic acid is added to neutralize for 30 min. Then, the product obtained in the reactor is taken out and added to a round-bottom flask, and then 6.1 g of water is added. Stirring is started at a speed of 1500 r / min to ensure that the materials are fully mixed.

[0062] (9) Weigh 84.1 g of hexamethylene diisocyanate, 0.5 g of tetramethylethylenediamine (catalyst) and 0.6 g of azodicarbonamide (foaming agent) and quickly add them into a round-bottom flask. Adjust the stirring speed of the stirrer to 3000 r / min. After 10 seconds, pour the mixed solution in the round-bottom flask into a mold that has been preheated to 40°C.

[0063] (10) The foam was allowed to stand in the mold for 30 min, and then the cured foam was placed in an oven at 80 °C to complete a 24 h curing process.

[0064] Comparative Example 1

[0065] (1) Weigh 34.7 g of hexachlorocyclotriphosphazene and dissolve it in 150 mL of toluene in a three-necked flask. Fix the three-necked flask in a constant temperature oil bath, install a condenser at one end, set the temperature to 120° C., so that the toluene refluxes, and start stirring to fully mix the materials.

[0066] (2) Weigh 44.8 g of triethanolamine and dissolve it in 50 mL of toluene. Add the mixture dropwise into a three-necked flask using a constant pressure dropping funnel and allow to react for 2 hours.

[0067] (3) After the reaction is completed, the temperature of the oil bath is adjusted to 85°C, 25.4 g of sodium bicarbonate is weighed and dissolved in deionized water, and the sodium bicarbonate solution is added to the system. A large number of bubbles are generated by the reaction. The reaction is continued for another 2 hours. When the reaction stops generating bubbles, the reaction is completed.

[0068] (4) After the reaction, adjust the temperature of the oil bath to 45°C, add an appropriate amount of dimethylformamide solvent to the product, stir thoroughly, and then let it stand for 1 hour.

[0069] (5) After standing for a period of time, granular salt product precipitates appear at the bottom of the bottle, and the upper liquid is separated for later use.

[0070] (6) Weigh 30 g of polyethylene glycol 300 and the separated upper liquid and add them to a jacketed reactor with a stirrer, and then add 1 ml of dibutyltin dilaurate. Pour an appropriate amount of heat transfer oil into the high-temperature circulator, connect the reactor, turn on the heating cycle of the high-temperature circulator, and set the temperature to 120°C. Then connect the jacketed reactor to a vacuum pump, turn on the vacuum pump, make the system pressure at 0.1 MPa, turn on the stirrer, accelerate the mixing of the materials, and evacuate for 2.5 hours.

[0071] (7) Without turning off the agitator and vacuum pump, adjust the temperature of the high-temperature circulator to 70°C, weigh 9.4 g of N-methyldiethanolamine, 3.5 g of 1,4-butanediol, and 1.8 g of trimethylolpropane. When the temperature of the reactor drops to 70°C, add the weighed chemicals into the reactor and continue the reaction for 2 hours.

[0072] (8) After the reaction is completed, the system is cooled to room temperature, and then 3.5 g of glacial acetic acid is added to neutralize for 30 min. Then, the product obtained in the reactor is taken out and added to a round-bottom flask, and then 2.4 g of water is added. Stirring is started at a speed of 1500 r / min to ensure that the materials are fully mixed.

[0073] (9) Weigh 42.0 g of hexamethylene diisocyanate, and then weigh 0.2 g of tetramethylethylenediamine (catalyst) and 0.2 g of azodicarbonamide (foaming agent) and quickly add them into a round-bottom flask. Adjust the stirring speed of the stirrer to 3000 r / min. After 10 seconds, pour the mixed solution in the round-bottom flask into a mold that has been preheated to 40°C.

[0074] (10) The foam was allowed to stand in the mold for 30 min, and then the cured foam was placed in an oven at 80 °C to complete a 24 h curing process.

[0075] Comparative Example 2

[0076] (1) Weigh 34.7 g of hexachlorocyclotriphosphazene and dissolve it in 150 mL of toluene in a three-necked flask. Fix the three-necked flask in a constant temperature oil bath, install a condenser at one end, set the temperature to 120° C., so that the toluene refluxes, and start stirring to fully mix the materials.

[0077] (2) Weigh 44.8 g of triethanolamine and dissolve it in 50 mL of toluene. Add the mixture dropwise into a three-necked flask using a constant pressure dropping funnel and allow to react for 2 hours.

[0078] (3) After the reaction is completed, the temperature of the oil bath is adjusted to 85°C, 50.4 g of sodium bicarbonate is weighed and dissolved in deionized water, and the sodium bicarbonate solution is added to the system to generate a large number of bubbles. The reaction is continued for another 2 hours until no bubbles are generated during the reaction, indicating that the reaction is complete.

[0079] (4) After the reaction, adjust the temperature of the oil bath to 45°C, add an appropriate amount of dimethylformamide solvent to the product, stir thoroughly, and then let it stand for 1 hour.

[0080] (5) After standing for a period of time, granular salt product precipitates appear at the bottom of the bottle, and the upper liquid is separated for later use.

[0081] (6) Weigh 30 g of polyethylene glycol 300 and the separated upper liquid and add them to a jacketed reactor with a stirrer, and then add 1 ml of dibutyltin dilaurate. Pour an appropriate amount of heat transfer oil into the high-temperature circulator, connect the reactor, turn on the heating cycle of the high-temperature circulator, and set the temperature to 120°C. Then connect the jacketed reactor to a vacuum pump, turn on the vacuum pump, make the system pressure at 0.1 MPa, turn on the stirrer, accelerate the mixing of the materials, and evacuate for 2.5 hours.

[0082] (7) Without turning off the agitator and vacuum pump, adjust the temperature of the high-temperature circulator to 70°C, weigh 18.8 g of N-methyldiethanolamine, 7.0 g of 1,4-butanediol, and 3.6 g of trimethylolpropane. When the temperature of the reactor drops to 70°C, add the weighed chemicals into the reactor and continue the reaction for 2 hours.

[0083] (8) After the reaction is completed, the system is cooled to room temperature, and then 3.5 g of glacial acetic acid is added to neutralize for 30 min. Then, the product obtained in the reactor is taken out and added to a round-bottom flask, and then 2.4 g of water is added. Stirring is started at a speed of 1500 r / min to ensure that the materials are fully mixed.

[0084] (9) Weigh 42.0 g of hexamethylene diisocyanate, and then weigh 0.2 g of tetramethylethylenediamine (catalyst) and 0.2 g of azodicarbonamide (foaming agent) and quickly add them into a round-bottom flask. Adjust the stirring speed of the stirrer to 3000 r / min. After 10 seconds, pour the mixed solution in the round-bottom flask into a mold that has been preheated to 40°C.

[0085] (10) The foam was allowed to stand in the mold for 30 min, and then the cured foam was placed in an oven at 80 °C to complete a 24 h curing process.

[0086] Performance Testing

[0087] The flame retardant polyurethane foams obtained in each embodiment and comparative example were tested for performance, and the results are shown in the following table:

[0088] Case Oxygen Index density Example 1 30% <![CDATA[0.036g / cm 2 ]]> Example 2 32% <![CDATA[0.038g / cm 2 ]]> Example 3 31% <![CDATA[0.040g / cm 2 ]]> Comparative Example 1 27% <![CDATA[0.039g / cm 2 ]]> Comparative Example 2 30% <![CDATA[0.022g / cm 2 ]]>

[0089] As shown in the table above, by comparing the embodiment with comparative example 1, it can be seen that adding insufficient amounts of sodium bicarbonate will reduce the limiting oxygen index of the polyurethane porous foam and deteriorate the flame retardant properties. This is because the main function of sodium bicarbonate is to remove the acidic substances produced in the first substitution reaction and promote the substitution reaction to move in the positive direction. Too little sodium bicarbonate will lead to incomplete reaction and decreased yield, thereby affecting the flame retardant properties of the subsequent polyurethane foam. By comparing the embodiment with comparative example 2, it can be seen that adding too much chain extender and cross-linking agent reduces the density of the polyurethane foam. Density is the most intuitive and simple data to characterize the quality of polyurethane foam. The strength and elastic modulus of polyurethane will increase significantly with the increase of its density. It can be seen from the density data that adding too much chain extender and cross-linking agent will seriously affect the mechanical properties of the polyurethane foam.

[0090] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0091] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a nitrogen-phosphorus flame-retardant modified polyurethane porous foam material, characterized in that The steps include: 1) adding hexachlorocyclotriphosphazene to an organic solvent, heating under reflux, stirring and mixing evenly, and then dropping triethanolamine to react; the molar ratio of triethanolamine to hexachlorocyclotriphosphazene is 2.5-3.5:1; 2) cooling, adding sodium bicarbonate solution to the reaction product of step 1) to neutralize the acid produced in step 1) and promote the substitution reaction to move forward; the molar ratio of sodium bicarbonate to hexachlorocyclotriphosphazene is 5-7:1; 3) After the reaction is completed, dimethylformamide solvent is added to the reaction product of step 2), and the mixture is heated and stirred; after standing, an equal amount of deionized water is added, and after a granular salt product precipitates at the bottom of the container, the upper layer solution is separated; 4) Add the upper solution, polyethylene glycol and catalyst to the reactor, heat at 110-130°C for 2-3h under vacuum and stirring conditions, then cool to 65-75°C, add chain extender A and chain extender B, internal crosslinker trimethylolpropane and solvent, and continue to react for 1.5-2.5h; The molar ratio of the polyethylene glycol to the hexachlorocyclotriphosphazene is (0.8-1.2):1; The amounts of chain extender A, chain extender B and internal crosslinking agent are 8-9%, 3-3.5% and 1.5-1.7% of the mass of the reaction system respectively; 5) After the reaction is completed, the system is cooled to room temperature, glacial acetic acid is added for neutralization, the product is taken out, water is added, hexamethylene diisocyanate, catalyst tetramethylethylenediamine and foaming agent azodicarbonamide are added, and after stirring evenly, the mixture is poured into a mold and allowed to stand for foaming; 6) After the foaming is completed, the polyurethane porous foam material is heated and aged to obtain a nitrogen-phosphorus flame-retardant modified polyurethane foam material.

2. The preparation method according to claim 1, characterized in that: In step 1), the reaction temperature is 130-150° C. and the reaction time is 1-3 h.

3. The preparation method according to claim 1 or 2, characterized in that: In step 1), the organic solvent is selected from one or more of acetone, toluene, xylene and tetrahydrofuran.

4. The preparation method according to claim 1, characterized in that: In step 2), the temperature after cooling is 80-90° C. and the reaction time is 1.5-2 h.

5. The preparation method according to claim 1, characterized in that: In step 3), The mass ratio of the dimethylformamide solvent to the hexachlorocyclotriphosphazene is 5-7:1; The heating and stirring is performed at a temperature of 40-50° C. and for a time of 0.5-1.5 h.

6. The preparation method according to claim 1, characterized in that: In step 4), The catalyst is dibutyltin dilaurate; The chain extender A is N-methyldiethanolamine; the chain extender B is 1,4-butanediol; The solvent is N-methylpyrrolidone.

7. The preparation method according to claim 1, characterized in that: In step 4), the pressure of the reactor is 0.08-0.12 MPa.

8. The preparation method according to claim 1, characterized in that: In step 5), The amount of glacial acetic acid added is 3-6wt% of the reaction system; the neutralization time is 20-40min; The amount of water added is 2-4wt% of the polyethylene glycol; The molar ratio of hexamethylene diisocyanate to hexachlorocyclotriphosphazene is 1:4-6; The amount of the catalyst tetramethylethylenediamine used is 0.1-0.2% of the mass of the reaction system; The amount of the foaming agent azodicarbonamide used is 0.1-0.3% of the mass of the reaction system.

9. The preparation method according to claim 1, characterized in that: In step 5), The stirring time is 5-15s; The mold is preheated at 35-45°C; The foaming is considered to be completed when the foam expands and solidifies in the mold.

10. The preparation method according to claim 1, characterized in that: In step 6), the aging temperature is 70-90° C. and the time is 20-30 hours.

Citation Information

Cited By

  • Preparation method of high-flame-retardance phosphazene-based polyether polyol

    CN121405922A