Multifunctional vegetable oil-based polyurethane soft foam as well as preparation method and application thereof

By using polyurethane flexible foam treated with biomass soybean oil polyol and MXene/PDMS, the problems of petrochemical resource dependence and poor electromagnetic shielding effect are solved, and environmentally friendly oil-water separation and efficient electromagnetic shielding effect are achieved.

CN118725239APending Publication Date: 2024-10-01INST OF CHEM IND OF FOREST PROD CHINESE ACAD OF FORESTRY

Patent Information

Application Number
CN202410713209.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing oil-water separation and electromagnetic shielding material preparation technologies have problems such as dependence on petrochemical resources, environmental pollution, and poor electromagnetic shielding effect.

Method used

Polyurethane flexible foam was prepared using biomass soybean oil polyol and polyether polyol, foaming agent, catalyst and foam stabilizer, and was impregnated with MXene and PDMS to prepare Ti3C2Tx-loaded multifunctional vegetable oil-based polyurethane flexible foam.

Benefits of technology

It achieves environmentally friendly oil-water separation and electromagnetic shielding, has super hydrophobicity and photothermal conversion properties, can effectively adsorb and recover high-viscosity crude oil, and achieves an electromagnetic shielding effect of about 33dB in the 8.2-12.4GHz band.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725239A_ABST
    Figure CN118725239A_ABST
Patent Text Reader

Abstract

The invention relates to multifunctional vegetable oil-based polyurethane soft foam and a preparation method and application thereof, biomass soybean oil polyol is used as a raw material and is uniformly mixed with polyether polyol, a foaming agent, a catalyst and a foam stabilizer, a component A precursor solution is prepared, component B isocyanate is added into the component A, the mixture is uniformly stirred, and the component B polyurethane soft foam is prepared. Foaming and curing to obtain polyurethane soft foam; the preparation method comprises the following steps: dipping polyurethane soft foam in an MXene (Ti3C2Tx) solution, carrying out ultrasonic treatment, taking out the polyurethane soft foam, and drying to obtain Ti3C2Tx-loaded polyurethane soft foam; and dipping the Ti3C2Tx-loaded polyurethane soft foam in a PDMS solution, carrying out ultrasonic treatment, and curing in a drying oven to obtain the multifunctional vegetable oil-based polyurethane soft foam. The obtained polyurethane soft foam has super-hydrophobicity, good photo-thermal conversion performance and good electromagnetic shielding effect, and can be used in the fields of crude oil adsorption and electromagnetic shielding; the preparation method is simple and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of bio-based polyurethane foam, and specifically relates to a multifunctional plant oil-based polyurethane soft foam and a preparation method and application thereof. Technical Background

[0002] With the continuous development of global industrialization, petroleum and chemical products have become the key driving force of global industrial growth. Large-scale offshore oil extraction, frequent ship transportation and escalating oil consumption have led to a surge in crude oil spills, posing a major threat to marine life and humans, and hindering the sustainable development of society. At the same time, the rapid development of the electronic information industry has brought great convenience to people, but it has also exposed serious electromagnetic pollution problems, becoming the fourth largest public hazard to human survival after noise pollution, air pollution and water pollution. The electromagnetic waves emitted by electronic and electrical equipment not only interfere with the normal operation of other instruments and equipment, but may also cause information leakage and even endanger human health.

[0003] At present, the raw materials for the production of commercial polyurethane foams used for oil-water separation mainly come from limited petrochemical resources, and the foams are usually directly discarded or incinerated after use, which will cause secondary pollution to the environment. Therefore, it is very necessary to find biomass resources to partially replace petrochemical resources to prepare biodegradable and environmentally friendly polyurethane soft foam oil-absorbing materials. Compared with commonly used petroleum-based polyols, vegetable oil polyols have the advantages of abundant raw material sources, low energy consumption, and good physical and chemical stability. At the same time, the main component of vegetable oil is triglyceride containing three long fatty chains. The double bonds, hydroxyl groups, epoxy groups and other functional groups in the molecules make their structure easy to modify, and they are the main source of synthetic bio-based polyols. Based on the above characteristics, vegetable oil has become the best biomass raw material for the preparation of bio-based polyurethane foam.

[0004] Traditional electromagnetic shielding materials, such as metal materials, have good electromagnetic shielding performance, but due to their own heavy weight, they cannot meet the current lightweight requirements. Polymer materials have become a research hotspot for the preparation of electromagnetic shielding materials due to their advantages such as light weight and easy molding and processing. A common method is to use materials with electromagnetic shielding properties as conductive fillers (such as carbon materials, metal powders and particles, etc.) and dope them with polymer matrices to form composite electromagnetic shielding materials. However, the conductive fillers have poor dispersibility and small addition amounts, resulting in low conductivity of the composite material and poor electromagnetic shielding effect; at the same time, due to the addition of conductive fillers, the mechanical properties of the composite material are greatly reduced compared to before addition, making it difficult to meet the design and subsequent processing requirements. The introduction of the pore structure of polyurethane soft foam can not only reduce the density of the material, but the pore wall can also serve as a reflection barrier for electromagnetic waves, improving the material's absorption performance for electromagnetic waves. Because of its three-dimensional skeleton structure, it can form an efficient conductive network, becoming an effective carrier for the preparation of efficient electromagnetic shielding materials. Summary of the invention

[0005] Technical problem to be solved: In view of the shortcomings of existing oil-water separation and electromagnetic shielding material preparation technologies, the present invention provides a multifunctional vegetable oil-based polyurethane soft foam and its preparation method and application. The polyurethane soft foam can be used for crude oil adsorption and has good electromagnetic shielding performance.

[0006] Technical solution: A method for preparing a multifunctional vegetable oil-based polyurethane soft foam, comprising the following steps: (1) using biomass soybean oil polyol as a raw material, mixing it with polyether polyol, foaming agent, catalyst and foam stabilizer to prepare component A, wherein the biomass soybean oil polyol is 20 to 60 parts, the polyether polyol is 40 to 80 parts, the foaming agent is 1.5 to 3 parts, the catalyst is 1.0 to 1.8 parts, and the foam stabilizer is 1.2 to 2.0 parts; adding component B isocyanate, 45 to 55 parts of isocyanate, to component A, and obtaining polyurethane soft foam after foaming and aging; (2) placing the polyurethane soft foam in a MXene (TiO2) film; and 3 C 2 T x ) solution and ultrasonically treated, and then the polyurethane soft foam was taken out and dried to obtain the loaded Ti 3 C 2 T x Polyurethane soft foam; (3) loading Ti 3 C 2 T x The polyurethane soft foam is immersed in 1-5wt.% PDMS n-hexane solution and ultrasonically treated, and then dried and solidified to obtain a multifunctional vegetable oil-based polyurethane soft foam.

[0007] Preferably, the weight proportions of the components in step (1) are as follows: 45 parts of soybean oil polyol, 55 parts of polyether polyol, 1.5-3 parts of foaming agent, 1.0-1.8 parts of catalyst, 1.2-2.0 parts of foam stabilizer; and 45-55 parts of isocyanate.

[0008] Preferably, the hydroxyl value of the soybean oil polyol in step (1) is 130 mg KOH·g -1 .

[0009] Preferably, the catalyst in step (1) is at least one of triethylenediamine, N-methylmorpholine, N-ethylmorpholine and stannous octoate.

[0010] Preferably, the foam stabilizer in step (1) is Maitu L580 or Maitu L-3881.

[0011] Preferably, the isocyanate in step (1) is toluene diisocyanate, diphenylmethane diisocyanate, polyphenylmethane polyisocyanate or isophorone diisocyanate.

[0012] Preferably, the MXene solution in step (2) is a single layer Ti 3 C 2 T x Suspension with a concentration of 0 to 25 mg mL -1 .

[0013] Preferably, in step (2), the ultrasonic treatment time is 0 to 2 hours, the vacuum drying oven temperature is 60 to 100° C., and the drying time is 1 to 3 hours; in step (3), the ultrasonic treatment time is 0 to 2 hours, the curing temperature is 60 to 100° C., and the curing time is 10 to 24 hours.

[0014] The multifunctional vegetable oil-based polyurethane soft foam is prepared by the method.

[0015] The multifunctional vegetable oil-based polyurethane soft foam is used in crude oil adsorption and electromagnetic shielding.

[0016] Beneficial effects: (1) The present invention uses soybean oil polyol derived from biomass resources to replace part of the petrochemical-based polyether polyol, and the prepared polyurethane soft foam is environmentally friendly;

[0017] (2) The plant oil-based polyurethane soft foam prepared in the present invention has super hydrophobicity and photothermal conversion performance, and can effectively realize the continuous in-situ adsorption and recovery of high-viscosity crude oil;

[0018] (3) The plant oil-based polyurethane soft foam prepared in the present invention has good electromagnetic shielding effectiveness, and can achieve a maximum shielding effect of about 33dB in the 8.2-12.4GHz band. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the full XPS spectrum of the foam materials prepared in Example 4 and Comparative Example 1;

[0020] Figure 2 This is a SEM image of the composite foam material prepared in Example 4;

[0021] Figure 3 The compressive stress-strain curves of the foam materials prepared in Example 4 and Comparative Example 1 under 70% strain conditions;

[0022] Figure 4 This is a graph showing the adsorption capacity of the composite foam material prepared in Example 4 over the illumination time;

[0023] Figure 5 Schematic diagram of the crude oil adsorption process of the composite foam material prepared in Example 4 under conditions of light and without light;

[0024] Figure 6This is a graph of the electromagnetic shielding effectiveness of the foam materials prepared in Example 4 and Comparative Examples 1-3. DETAILED DESCRIPTION

[0025] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the spirit and essence of the present invention, modifications and substitutions made to the method, steps or conditions of the present invention all belong to the scope of the present invention. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art.

[0026] Example 1

[0027] Single layer Ti 3 C 2 T x Preparation:

[0028] Step 1: Add 1.85 g LiF to 40 mL 9 M hydrochloric acid solution and stir for 10 min (500 r / min) in an ice bath. -1 ) to obtain a uniform etching solution;

[0029] Step 2: Add 1.9g MAX(Ti 3 AlC 2 , 400 mesh, purchased from Foshan Xinxin Technology Co., Ltd.), and stirred and reacted at 35 °C for 24 h to obtain a multilayer MXene solution;

[0030] Step 3: The obtained solution was heated at 4000 r / min -1 Centrifuge for 5 minutes, wash repeatedly with deionized water 5-6 times, and ultrasonicate for 1 hour; repeat centrifugation and add water to repeatedly peel off the lower sediment until a dark green Ti 3 C 2 T x Suspension, collect the prepared monolayer MXene solution, determine the solid content, and prepare it to a concentration of 5 mg mL -1 , 10mg·mL -1 , 15mg·mL -1 , 20mg·mL -1 and 25 mg mL -1 The solution is ready for use.

[0031] Example 2

[0032] Step 1: 45 parts of hydroxyl value 130 mg KOH g -1 55 parts of soybean oil polyol were mixed with 55 parts of polyether polyol in proportion, 2.0 parts of deionized water as a foaming agent, 0.8 parts of triethylene diamine, 0.6 parts of stannous octoate and 1.6 parts of foam stabilizer Momentive L580 were added, and the mixture was stirred at 800 r / min. -1The precursor solution of component A was prepared by stirring for 3 minutes at a speed of 2000 r·min, and 52.8 parts of diphenylmethane diisocyanate were added thereto. -1 The mixture was stirred at a speed of 5000 s for natural foaming and aged at 60°C for 2 h to obtain polyurethane soft foam;

[0033] Step 2: Place polyurethane soft foam in a solution with a concentration of 5 mg mL -1 MXene(Ti 3 C 2 T x ) solution and ultrasonically treated for 1 h, then the polyurethane soft foam was taken out and placed in a vacuum drying oven at 80 °C for 2 h to obtain the loaded Ti 3 C 2 T x Polyurethane soft foam;

[0034] Step 3: First, PDMS and curing agent were mixed in a mass ratio of 10:1 and dissolved in n-hexane to prepare a 1 wt.% PDMS n-hexane solution. 3 C 2 T x The polyurethane soft foam was immersed in 1wt.% PDMS n-hexane solution and ultrasonically treated for 1h, and then cured in an oven at 80°C for 12h to obtain a multifunctional vegetable oil-based polyurethane soft foam.

[0035] Example 3

[0036] Step 1: 45 parts of hydroxyl value 130 mg KOH g -1 55 parts of soybean oil polyol were mixed with 55 parts of polyether polyol in proportion, 2.0 parts of deionized water as a foaming agent, 0.8 parts of triethylene diamine, 0.6 parts of stannous octoate and 1.6 parts of foam stabilizer Momentive L580 were added, and the mixture was stirred at 800 r / min. -1 The precursor solution of component A was prepared by stirring for 3 minutes at a speed of 2000 r·min, and 52.8 parts of diphenylmethane diisocyanate were added thereto. -1 The mixture was stirred at a speed of 5000 s for natural foaming and aged at 60°C for 2 h to obtain polyurethane soft foam;

[0037] Step 2: Place polyurethane soft foam in a solution with a concentration of 10 mg mL -1 MXene(Ti 3 C 2 T x ) solution and ultrasonically treated for 1 h, then the polyurethane soft foam was taken out and placed in a vacuum drying oven at 80 °C for 2 h to obtain the loaded Ti 3 C 2 T x Polyurethane soft foam;

[0038] Step 3: First, PDMS and curing agent were mixed in a mass ratio of 10:1 and dissolved in n-hexane to prepare a 1 wt.% PDMS n-hexane solution. 3 C 2 T x The polyurethane soft foam was immersed in 1wt.% PDMS n-hexane solution and ultrasonically treated for 1h, and then cured in an oven at 80°C for 12h to obtain a multifunctional vegetable oil-based polyurethane soft foam.

[0039] Example 4

[0040] Step 1: 45 parts of hydroxyl value 130 mg KOH g -1 55 parts of soybean oil polyol were mixed with 55 parts of polyether polyol in proportion, 2.0 parts of deionized water as a foaming agent, 0.8 parts of triethylene diamine, 0.6 parts of stannous octoate and 1.6 parts of foam stabilizer Momentive L580 were added, and the mixture was stirred at 800 r / min. -1 The precursor solution of component A was prepared by stirring for 3 minutes at a speed of 2000 r·min, and 52.8 parts of diphenylmethane diisocyanate were added thereto. -1 The mixture was stirred at a speed of 5000 s for natural foaming and aged at 60°C for 2 h to obtain polyurethane soft foam;

[0041] Step 2: Place polyurethane soft foam in a solution with a concentration of 15 mg mL -1 MXene(Ti 3 C 2 T x ) solution and ultrasonically treated for 1 h, then the polyurethane soft foam was taken out and placed in a vacuum drying oven at 80 °C for 2 h to obtain the loaded Ti 3 C 2 T x Polyurethane soft foam;

[0042] Step 3: First, PDMS and curing agent were mixed in a mass ratio of 10:1 and dissolved in n-hexane to prepare a 1 wt.% PDMS n-hexane solution. 3 C 2 T x The polyurethane soft foam was immersed in 1wt.% PDMS n-hexane solution and ultrasonically treated for 1h, and then cured in an oven at 80°C for 12h to obtain a multifunctional vegetable oil-based polyurethane soft foam.

[0043] Example 5

[0044] Step 1: 45 parts of hydroxyl value 130 mg KOH g -155 parts of soybean oil polyol were mixed with 55 parts of polyether polyol in proportion, 2.0 parts of deionized water as a foaming agent, 0.8 parts of triethylene diamine, 0.6 parts of stannous octoate and 1.6 parts of foam stabilizer Momentive L580 were added, and the mixture was stirred at 800 r / min. -1 The precursor solution of component A was prepared by stirring for 3 minutes at a speed of 2000 r·min, and 52.8 parts of diphenylmethane diisocyanate were added thereto. -1 The mixture was stirred at a speed of 5000 s for natural foaming and aged at 60°C for 2 h to obtain polyurethane soft foam;

[0045] Step 2: Place polyurethane soft foam in a solution with a concentration of 20 mg mL -1 MXene(Ti 3 C 2 T x ) solution and ultrasonically treated for 1 h, then the polyurethane soft foam was taken out and placed in a vacuum drying oven at 80 °C for 2 h to obtain the loaded Ti 3 C 2 T x Polyurethane soft foam;

[0046] Step 3: First, PDMS and curing agent were mixed in a mass ratio of 10:1 and dissolved in n-hexane to prepare a 1 wt.% PDMS n-hexane solution. 3 C 2 T x The polyurethane soft foam was immersed in 1wt.% PDMS n-hexane solution and ultrasonically treated for 1h, and then cured in an oven at 80°C for 12h to obtain a multifunctional vegetable oil-based polyurethane soft foam.

[0047] Example 6

[0048] Step 1: 45 parts of hydroxyl value 130 mg KOH g -1 55 parts of soybean oil polyol were mixed with 55 parts of polyether polyol in proportion, 2.0 parts of deionized water as a foaming agent, 0.8 parts of triethylene diamine, 0.6 parts of stannous octoate and 1.6 parts of foam stabilizer Momentive L580 were added, and the mixture was stirred at 800 r / min. -1 The precursor solution of component A was prepared by stirring for 3 minutes at a speed of 2000 r·min, and 52.8 parts of diphenylmethane diisocyanate were added thereto. -1 The mixture was stirred at a speed of 5000 s for natural foaming and aged at 60°C for 2 h to obtain polyurethane soft foam;

[0049] Step 2: Place polyurethane soft foam in a solution with a concentration of 25 mg mL -1 MXene(Ti 3 C 2 T x) solution and ultrasonically treated for 1 h, then the polyurethane soft foam was taken out and placed in a vacuum drying oven at 80 °C for 2 h to obtain the loaded Ti 3 C 2 T x Polyurethane soft foam;

[0050] Step 3: First, PDMS and curing agent were mixed in a mass ratio of 10:1 and dissolved in n-hexane to prepare a 1 wt.% PDMS n-hexane solution. 3 C 2 T x The polyurethane soft foam was immersed in 1wt.% PDMS n-hexane solution and ultrasonically treated for 1h, and then cured in an oven at 80°C for 12h to obtain a multifunctional vegetable oil-based polyurethane soft foam.

[0051] Comparative Example 1

[0052] Step 1: 45 parts of hydroxyl value 130 mg KOH g -1 55 parts of soybean oil polyol were mixed with 55 parts of polyether polyol in proportion, 2.0 parts of deionized water as a foaming agent, 0.8 parts of triethylene diamine, 0.6 parts of stannous octoate and 1.6 parts of foam stabilizer Momentive L580 were added, and the mixture was stirred at 800 r / min. -1 The precursor solution of component A was prepared by stirring for 3 minutes at a speed of 2000 r·min, and 52.8 parts of diphenylmethane diisocyanate were added thereto. -1 The mixture was stirred at a speed of 5000 nm for 5 seconds, foamed naturally, and aged at 60°C for 2 hours to obtain polyurethane soft foam.

[0053] Comparative Example 2

[0054] Step 1: 45 parts of hydroxyl value 130 mg KOH g -1 55 parts of soybean oil polyol were mixed with 55 parts of polyether polyol in proportion, 2.0 parts of deionized water as a foaming agent, 0.8 parts of triethylene diamine, 0.6 parts of stannous octoate and 1.6 parts of foam stabilizer Momentive L580 were added, and the mixture was stirred at 800 r / min. -1 The precursor solution of component A was prepared by stirring for 3 minutes at a speed of 2000 r·min, and 52.8 parts of diphenylmethane diisocyanate were added thereto. -1 The mixture was stirred at a speed of 5000 s for natural foaming and aged at 60°C for 2 h to obtain polyurethane soft foam;

[0055] Step 2: First, PDMS and curing agent were mixed in a mass ratio of 10:1 and dissolved in n-hexane to prepare a 1 wt.% PDMS n-hexane solution. 2 C 3 T xThe polyurethane flexible foam was immersed in 1 wt.% PDMS n-hexane solution and ultrasonically treated for 1 h, and then cured in an oven at 80°C for 12 h to obtain a vegetable oil-based polyurethane flexible foam cured only with PDMS.

[0056] Comparative Example 3

[0057] Step 1: 45 parts of hydroxyl value 130 mg KOH g -1 55 parts of soybean oil polyol were mixed with 55 parts of polyether polyol in proportion, 2.0 parts of deionized water as a foaming agent, 0.8 parts of triethylene diamine, 0.6 parts of stannous octoate and 1.6 parts of foam stabilizer Momentive L580 were added, and the mixture was stirred at 800 r / min. -1 The precursor solution of component A was prepared by stirring for 3 minutes at a speed of 2000 r·min, and 52.8 parts of diphenylmethane diisocyanate were added thereto. -1 The mixture was stirred at a speed of 5000 s for natural foaming and aged at 60°C for 2 h to obtain polyurethane soft foam;

[0058] Step 2: Place polyurethane soft foam in a solution with a concentration of 15 mg mL -1 MXene(Ti 3 C 2 T x ) solution and ultrasonically treated for 1 h, then the polyurethane soft foam was taken out and placed in a vacuum drying oven at 80 °C for 2 h to obtain a polyurethane foam loaded with Ti 3 C 2 T x Polyurethane soft foam.

[0059] Table 1 Comparison of properties of multifunctional vegetable oil-based polyurethane soft foams prepared in various embodiments

[0060]

[0061]

[0062] It can be seen from Table 1 that the water contact angle of the multifunctional plant oil-based polyurethane soft foam prepared by the present invention is 153.3°~160.4°, and the electromagnetic shielding effectiveness in the 8.2~12.4GHz band is 9.78~33.35dB. Among them, Example 4 has the best comprehensive performance, with a contact angle of 160.4°. The mechanical properties test is carried out under 70% strain conditions, and the compressive stress can reach 60.82KPa, and the electromagnetic shielding effectiveness can reach 28.24dB.

[0063] The polyurethane foams prepared in Example 4 and Comparative Example 1 were subjected to elemental comparative analysis. The results are as follows: Figure 1 As shown in the figure, Example 4 not only contains the basic elements C, O, and Si, but also the characteristic elements Ti and F, indicating that Ti 3C 2 T x The composite foam was successfully loaded on the foam surface; the SEM image of the composite foam is shown in Figure 2 As shown, the uniform rough structure on the foam surface further indicates that Ti 3 C 2 T x of successful load.

[0064] The mechanical properties of the polyurethane foams prepared in Example 4 and Comparative Example 1 were analyzed. Figure 3 As shown, under the condition of 70% strain, the compressive stress of Example 4 is significantly improved compared with that of Comparative Example 1 (24.69 KPa), and the embodiment 4 has excellent mechanical properties, thereby improving the recyclability of the polyurethane soft foam.

[0065] The adsorption capacity of the polyurethane foams prepared in Example 4 and Comparative Example 1 was compared and analyzed. The results are as follows: Figure 4 As shown in Figure 2, under simulated light conditions, the adsorption capacity of Example 4 can reach 12.10 g·g -1 , which can quickly carry out photothermal conversion, reduce crude oil viscosity and quickly adsorb crude oil. The schematic diagram of the crude oil adsorption process with and without light conditions is shown in the figure. Figure 5 shown.

[0066] The polyurethane foams prepared in Example 4 and Comparative Examples 1-3 were tested for electromagnetic shielding effectiveness. The results are as follows: Figure 6 As shown, the electromagnetic shielding effectiveness of the composite foam prepared in Example 4 is significantly improved compared with that in Comparative Example 1, and Comparative Examples 2 and 3 have the lowest and best electromagnetic shielding effectiveness, respectively.

[0067] The present invention uses widely available and renewable vegetable oil polyols as raw materials to replace part of petrochemical resources to prepare polyurethane foam, which is environmentally friendly. 3 C 2 T x Compared with unmodified foam, the polyurethane soft foam cured with PDMS has excellent mechanical properties and super hydrophobicity, and can perform continuous oil-water separation; the prepared polyurethane soft foam has excellent photothermal conversion performance, and can effectively achieve continuous in-situ adsorption and recovery of high-viscosity crude oil under illumination conditions; at the same time, the polyurethane soft foam has good electromagnetic shielding effectiveness, and the electromagnetic shielding effectiveness can reach 28.24dB when the comprehensive performance is optimal. The vegetable oil-based polyurethane soft foam proposed by the present invention integrates multiple functions and broadens the scope of application of the polyurethane soft foam.

Claims

1. A method for preparing a multifunctional vegetable oil-based polyurethane soft foam, characterized in that: The following steps are involved: (1) Biomass soybean oil polyol is used as a raw material, and is evenly mixed with polyether polyol, foaming agent, catalyst and foam stabilizer to prepare component A, wherein the biomass soybean oil polyol is 20-60 parts, the polyether polyol is 40-80 parts, the foaming agent is 1.5-3 parts, the catalyst is 1.0-1.8 parts, and the foam stabilizer is 1.2-2.0 parts; Component B isocyanate is added to component A, and the isocyanate is 45-55 parts. After foaming and aging, a polyurethane soft foam is obtained; (2) The polyurethane soft foam is placed in MXene (Ti3C2T x ) solution and ultrasonically treated, and then the polyurethane soft foam was taken out and dried to obtain the loaded Ti3C2T x Polyurethane soft foam; (3) Loading Ti3C2T x The polyurethane soft foam was immersed in 1~5wt.% PDMS n-hexane solution and ultrasonically treated, and then dried and solidified to obtain a multifunctional vegetable oil-based polyurethane soft foam.

2. The method for preparing the multifunctional vegetable oil-based polyurethane soft foam according to claim 1, characterized in that: The weight proportions of the components in step (1) are as follows: 45 parts of soybean oil polyol, 55 parts of polyether polyol, 1.5-3 parts of foaming agent, 1.0-1.8 parts of catalyst, 1.2-2.0 parts of foam stabilizer; and 45-55 parts of isocyanate.

3. The method for preparing the multifunctional vegetable oil-based polyurethane soft foam according to claim 1, characterized in that: The hydroxyl value of soybean oil polyol in step (1) is 130 mg KOH g -1 .

4. The method for preparing the multifunctional vegetable oil-based polyurethane soft foam according to claim 1, characterized in that: The catalyst in step (1) is at least one of triethylenediamine, N-methylmorpholine, N-ethylmorpholine and stannous octoate.

5. The method for preparing the multifunctional vegetable oil-based polyurethane soft foam according to claim 1, characterized in that: The foam stabilizer in step (1) is Maitu L580 or Maitu L-3881.

6. The method for preparing the multifunctional vegetable oil-based polyurethane soft foam according to claim 1, characterized in that: In step (1), the isocyanate is toluene diisocyanate, diphenylmethane diisocyanate, polyphenylmethane polyisocyanate or isophorone diisocyanate.

7. The method for preparing the multifunctional vegetable oil-based polyurethane soft foam according to claim 1, characterized in that: The MXene solution in step (2) is a single layer Ti3C2T x Suspension with a concentration of 5-25 mg mL -1 .

8. The method for preparing the multifunctional vegetable oil-based polyurethane soft foam according to claim 1, characterized in that: In step (2), the ultrasonic treatment time is 0 to 2 h, the vacuum drying oven temperature is 60 to 100° C., and the drying time is 1 to 3 h. In step (3), the ultrasonic treatment time is 0 to 2 h, the curing temperature is 60 to 100° C., and the curing time is 10 to 24 h.

9. The multifunctional vegetable oil-based polyurethane soft foam prepared according to any one of claims 1 to 8.

10. Use of the multifunctional vegetable oil-based polyurethane soft foam according to claim 9 in crude oil adsorption and electromagnetic shielding.

Citation Information

Patent Citations

  • Three-dimensional layered MXene electromagnetic shielding foam and preparation method thereof

    CN108811478A

  • Preparation method of electromagnetic shielding type polyurethane lightweight material

    CN109942877A

  • Flexible conductive MXene-based foam and preparation method thereof

    CN111286078A

  • Polyurethane flexible foamed plastic and preparation method thereof

    CN112062927A

  • Polyurethane flexible foam and preparation method thereof

    CN114249873A

Cited By

  • Bio-based flame-retardant flexible polyurethane foam with photo-thermal conversion performance as well as preparation method and application of bio-based flame-retardant flexible polyurethane foam

    CN119570108A