Solar evaporator based on porous polypyrrole, preparation method of solar evaporator and application of solar evaporator in nano plastic sewage purification
Through solar evaporators based on porous polypyrrole, utilizing its photothermal properties and hydrophilicity, the problem of separation of nanoplastic pollution in water bodies is solved, efficient water purification and nanoplastic removal are achieved, and a simple and low-cost solution is provided. solution.
Patent Information
- Application Number
- CN202410937587.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
AI Technical Summary
Existing technology is difficult to effectively remove nanoplastic pollution in water, especially during the purification process, the separation effect of nanoplastics from clean water vapor is not good, and the commonly used adsorption method has the problem of reduced purification speed.
Using a solar evaporator based on porous polypyrrole, porous polypyrrole is constructed through in-situ polymerization of pyrrole and ferric chloride hexahydrate, and its excellent photothermal properties and hydrophilicity are used to convert solar energy into thermal energy within the solar spectrum. Evaporation of water and separation of nanoplastics.
Efficient separation of nanoplastics and clean water is achieved, with an evaporation rate of 2.339kg·m-2·h-1 and a solar steam conversion efficiency of 89.6%. The purification method is simple and low-cost, suitable for industrial promotion and does not require additional energy.
Smart Images

Figure CN118725294A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photothermal materials, and in particular to a solar evaporator based on porous polypyrrole, a preparation method thereof, and application thereof in nano-plastic wastewater purification. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] With the development of industry, plastic products are being widely used in various industries, such as packaging, building materials, daily personal care products, vehicles, clothing and electronic products. When plastics enter water bodies through sewage discharge and surface runoff, some larger plastics are decomposed into nanoplastics with smaller particle sizes (1-100nm) through weathering, biodegradation, photodegradation and thermal degradation. Due to the tiny size of nanoplastics, they are easily swallowed and ingested by organisms and accumulated along the food chain. In addition, nanoplastics have large specific surface area, complex surface properties, good resistance to degradation, and show excellent ability in adsorbing, concentrating and transporting toxic compounds. Therefore, nanoplastic pollution in water bodies has become an increasingly serious environmental problem.
[0004] At present, the main methods for treating nanoplastics in water bodies include adsorption by adsorbents and coagulation and sedimentation. Among them, the adsorption method is considered to be one of the most promising methods due to its simple operation and low cost. However, the adsorbent in the adsorption method will gradually become blocked as the adsorption proceeds, reducing the purification speed.
[0005] Solar interfacial water evaporation is an emerging solar-driven water treatment technology that uses the photothermal effect to cause water to evaporate on the surface of porous materials, thereby achieving water purification. However, there are no reports on the use of solar interfacial evaporation to remove nanoplastics from water. Summary of the invention
[0006] In order to overcome the above problems, the present invention provides a solar evaporator based on porous polypyrrole, a preparation method thereof and its application in nanoplastic wastewater purification. The porous polypyrrole provided by the present invention has good light absorption performance in the entire solar spectrum, and has a high evaporation rate and solar steam conversion efficiency, so it can be used as a solar evaporator. The solar evaporator based on porous polypyrrole provided by the present invention can effectively remove nanoplastics in water and achieve water purification.
[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0008] The first aspect of the present invention provides a method for preparing porous polypyrrole, comprising:
[0009] The pyrrole solution and the ferric chloride solution are mixed, heated for polymerization, and allowed to stand at room temperature after the reaction is completed to obtain porous polypyrrole.
[0010] In one or more embodiments, the concentration of the pyrrole solution is 0.8 to 1.2 mol / L, preferably 1 mol / L.
[0011] In one or more embodiments, the ferric chloride is ferric chloride hexahydrate; the concentration of the ferric chloride hexahydrate solution is 0.8-1.2 mol / L, preferably 1 mol / L.
[0012] In one or more embodiments, the molar ratio of pyrrole to ferric chloride is 0.9 to 1.2:1, preferably 1:1.
[0013] In one or more embodiments, the temperature of the heating polymerization is 55 to 65° C., preferably 60° C.; the time of the heating polymerization is 0.5 to 1.5 h, preferably 1 h.
[0014] In one or more embodiments, the standing time at room temperature is 20 to 30 hours, preferably 24 hours.
[0015] The second aspect of the present invention provides porous polypyrrole prepared by the above preparation method.
[0016] In one or more embodiments, the pore size of the porous polypyrrole is 3 to 40 μm.
[0017] The third aspect of the present invention provides a solar evaporator, which comprises the porous polypyrrole. The porous polypyrrole provided by the present invention has good light absorption performance in the entire solar spectrum as a photothermal material, and can convert solar energy into heat energy for photothermal evaporation, so it can be used as a solar evaporator.
[0018] The fourth aspect of the present invention provides use of the porous polypyrrole described in the first aspect and / or the solar evaporator described in the third aspect in water treatment.
[0019] In one or more embodiments, the water treatment includes seawater evaporation and sewage treatment.
[0020] Preferably, the sewage treatment includes acid-base sewage purification, organic dye sewage purification and nano-plastic sewage purification.
[0021] Further preferably, the organic dye comprises rhodamine b, Congo red and bromophenol blue.
[0022] The beneficial effects of the present invention are:
[0023] (1) The present invention constructs porous polypyrrole by in-situ polymerization of pyrrole and ferric chloride hexahydrate, and the porous polypyrrole has excellent photothermal properties, good hydrophilicity and abundant pores. The porous polypyrrole provided by the present invention is used as a photothermal material, has good light absorption performance in the entire solar spectrum, and can convert solar energy into thermal energy for photothermal evaporation, so it can be used as a solar evaporator. At the same time, good hydrophilicity and abundant pores can accelerate the adsorption and evaporation of water, so that it has a higher evaporation rate and solar steam conversion efficiency; specifically, when the porous polypyrrole is used as a solar evaporator, the evaporation rate can reach 2.339 kg·m under 1 standard solar radiation intensity. -2 ·h -1 , the solar steam conversion efficiency can reach 89.6%.
[0024] (2) During the evaporation purification process, wastewater containing nanoplastics is continuously transported to the evaporation interface. Since porous polypyrrole has an excellent photothermal effect, it can absorb solar energy at the evaporation interface and convert it into heat energy, generating convective lift, thereby moving water vapor upward. However, since the density of nanoplastics is much greater than the density of air, convective lift cannot lift them upward, and the nanoplastics will remain in the wastewater, thereby achieving the separation of nanoplastics from clean water vapor.
[0025] (3) The present invention uses a porous polypyrrole solar evaporator to directly separate nanoplastics and water in wastewater containing nanoplastics, and only needs the sun for energy supply, without requiring additional energy. The purification method is simple, low-cost, clean and efficient, and easy to promote in industry.
[0026] (4) The present invention combines the removal of nanoplastics with solar interface evaporation, which has great potential in alleviating nanoplastic pollution and water shortage. In addition, the method for removing nanoplastics provided by the present invention will also open up new avenues for the development of nanoplastic removal technology and the application of solar interface evaporation technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0028] Figure 1 The synthesis process of porous polypyrrole in Example 1;
[0029] Figure 2 is a scanning electron microscope image of porous polypyrrole;
[0030] Figure 3 The infrared spectra of pyrrole, ferric chloride hexahydrate and porous polypyrrole;
[0031] Figure 4 is the pore size distribution diagram of porous polypyrrole;
[0032] Figure 5 a is the absorption spectrum of porous polypyrrole and AM 1.5G (blue-purple region); b is the reflection spectrum of porous polypyrrole;
[0033] Figure 6 Porous polypyrrole water drop contact angle test;
[0034] Figure 7 It is a simple condensed water collection device;
[0035] Figure 8 a is the ion concentration of the Yellow Sea water and the treated seawater; b is the photo of the flat plate coating of the Yellow Sea water and the treated seawater; c is the resistance of the sample measured by a multimeter (the distance between the electrodes remains unchanged);
[0036] Fig. 9 This is a picture of pH test paper before and after purification of strong acid and strong base solutions;
[0037] Fig.10 UV spectra of Rhodamine B, Congo red, and bromophenol blue simulated wastewater before and after purification. Inset: Color changes of simulated wastewater before (left) and after (right) purification.
[0038] Fig.11 Laser confocal images of tomato root, stem and fruit slices cultivated for water purification and nanoplastic contaminated water;
[0039] Fig.12 These are transmission electron microscope photos of pure water, nanoplastic contaminated water in the nanoplastic group, purified water collected after evaporation purification by a porous polypyrrole system, and purified remaining water in a beaker. From left to right, they are the purified remaining water in the beaker after evaporation purification of nanoplastic contaminated water in the nanoplastic group by a porous polypyrrole system, pure water, and purified water collected after evaporation purification by a porous polypyrrole system. DETAILED DESCRIPTION
[0040] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0041] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0042] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0043] In Experimental Example 1, PS-NPs with green fluorescence were purchased from Tianjin Bestle Chromatography Technology Development Center, Lumisphere fluorescent microspheres, Green Fluorescent Microspheres, product number 7-3-0008, and size was 0.08 microns.
[0044] Example 1
[0045] Figure 1 In the synthesis process of porous polypyrrole, 10 mL of 1 M pyrrole solution and 10 mL of 1 M ferric chloride hexahydrate solution were mixed in a beaker and placed in a 60°C oven for polymerization. After 1 hour, the mixture was taken out and allowed to stand at room temperature for 24 hours. After the standing was completed, the porous polypyrrole was taken out and cut into 1×1×1 cm cubes, which were the solar evaporator.
[0046] The microstructure of porous polypyrrole was characterized by scanning electron microscopy. Figure 2 As shown, from Figure 1 It can be seen that the surface of porous polypyrrole is rough and has dense holes, and the diameter of these holes is about 10μm. These holes are interconnected inside the porous polypyrrole to form an irregular network structure. The capillary force generated can transport water from the interface to the photothermal surface and effectively ensure the escape of water vapor. At the same time, sunlight is also reflected multiple times in these irregular holes, and finally absorbed and converted into heat inside the polypyrrole, thereby reducing the waste of solar energy caused by reflection, diffuse reflection, etc.
[0047] Fourier transform infrared spectroscopy (FTIR) was used to characterize pyrrole, ferric chloride hexahydrate and porous polypyrrole. Figure 3 As shown, polypyrrole and pyrrole are at 3350 cm -1 The characteristic peaks appearing near are attributed to the stretching vibration of NH. Compared with ferric chloride hexahydrate and pyrrole, the infrared characteristic peaks unique to polypyrrole appear at 1519 cm -1This is due to the stretching vibration of CN in the pyrrole ring. The appearance of this characteristic peak proves that polypyrrole has been successfully synthesized. -1 and 1000cm -1 The typical bands at are caused by the CC intra-ring stretching and CH plane bending vibrations of the pyrrole ring.
[0048] The pore size distribution of porous polypyrrole was characterized by mercury porosimetry. Figure 4 As shown, the pore size is mainly distributed in the range of 3 to 40 μm, which is consistent with the results of surface scanning by SEM. The porous structure of porous polypyrrole is an important condition for ensuring water transport and light absorption.
[0049] Good photothermal performance is an important factor for the excellent performance of solar evaporators. Ultraviolet-visible-near infrared spectroscopy (UV-vis-NIR) was used to measure the light absorption performance of porous polypyrrole. Figure 5 As shown in the figure, porous polypyrrole exhibits excellent stability and light absorption performance in the wavelength range of 200-2500nm. Compared with the standard solar spectrum (airmass 1.5global, AM 1.5G), the absorptivity of polypyrrole is about 98.6% and the reflectivity is about 1.4% in the full wavelength range. This is mainly due to the intricate bundle structure inside the polypyrrole, which not only prolongs the path of light transmission, but also causes multiple reflections of light inside the bundle, reducing the energy loss caused by reflection and diffuse reflection.
[0050] To ensure the continuity of the evaporation process, the solar evaporator must have a good water transport capacity from the bulk water to the evaporation interface. To explore the hydrophilicity of porous polypyrrole, a video optical contact angle meter was used to measure it. The results are shown in Figure 6 As shown in the figure, polypyrrole monomer can absorb all water droplets in 30ms, which is mainly due to the hydrophilic groups and complex internal structure of polypyrrole. This provides a basis for achieving stable and continuous water evaporation of polypyrrole monomer.
[0051] Solar steam generation experimental characterization: The porous polypyrrole solar evaporator prepared in this example can generate 2.339 kg·m of pure water under 1 standard solar radiation intensity. -2 ·h -1 , the solar steam conversion efficiency can reach 89.6%.
[0052] Experimental Example 1
[0053] Use Figure 7The simple condensate collection device is used to perform seawater desalination, acid-base wastewater purification, organic wastewater purification and nano-plastic wastewater purification experiments on the solar evaporator provided in Example 1. The condensate collection device includes a large culture dish at the bottom, a small beaker is placed in the large culture dish, and a large beaker is placed outside the small beaker.
[0054] The specific test process is as follows: pour an appropriate amount of seawater, acid-base organic wastewater purification or nano-plastic wastewater into a small beaker; open a through hole in the center of the foam with a diameter smaller than the small beaker, and the side length of the through hole is slightly smaller than the porous polypyrrole solar evaporator. The porous polypyrrole solar evaporator is just embedded in the through hole and will not fall off. Place the foam with the porous polypyrrole solar evaporator on the water surface, and then cover the large beaker on the upper part of the small beaker and place it under an artificial solar lamp; condensed water will gather on the large beaker and remain along the inner wall of the large beaker, and finally the condensed water can be collected on the large culture dish at the bottom.
[0055] 1.1 Determination of K in the condensed water after purification of the Yellow Sea by ICP-OES + , Ca 2+ 、Na + and Mg 2+ The concentration of four ions related to drinking water quality. Figure 8 As shown in a, K + , Ca 2+ 、Na + and Mg 2+ 0.49mg L-1, 9.28mg L-1 respectively -1 , 22.52mg L -1 , 0.55mg L -1 The ion concentrations of seawater purified by the porous polypyrrole solar evaporator are far lower than the standard values of ion concentration for drinking water stipulated by WHO and EPA, and have good drinking quality for human body.
[0056] To further evaluate the safety of the treated seawater from the Yellow Sea, the seawater before and after treatment was spread on plate count medium (PCA). Figure 8 As shown in b, a large number of colonies grew on the culture medium coated with the Yellow Sea water before purification, while no colonies were found on the culture medium coated with the purified seawater after purification by the polypyrrole solar evaporator, which indicates that microorganisms were removed during the evaporation purification process of the Yellow Sea water.
[0057] The electrical resistance of water can reflect the water quality. The purer the water, the higher the conductivity and the greater the resistance. The electrical conductivity of the Yellow Sea seawater, purified water and domestic water was measured to test the purity of the water. The results are as follows: Figure 8As shown in c, the resistance of seawater before and after treatment and the resistance of domestic water are 110KΩ, 1.079MΩ, and 632KΩ respectively. The water purified by the polypyrrole evaporator has the highest resistance, which shows that the purification of seawater by the polypyrrole evaporator improves the water quality, and the purified water can be used as daily water.
[0058] 1.2 In order to fully study the application potential of polypyrrole evaporator in water purification, strong acid solution with pH 1.0 and strong alkaline solution with pH 14.0 were selected as purification objects. Fig. 9 As shown, the water obtained after the strong acid and strong base solutions are purified by the polypyrrole evaporator is close to neutral, which proves that the polypyrrole evaporator has good acid and alkali purification capabilities.
[0059] 1.3 In order to investigate the ability of polypyrrole monomer evaporator to purify wastewater containing organic dyes, rhodamine b solution (mass fraction 0.5%), Congo red solution (mass fraction 0.5%) and bromophenol blue solution (mass fraction 0.5%) were selected as pollutant models and added into deionized water for testing. The results are shown in Fig.10 As shown in the figure, the purified liquid becomes colorless, and its absorbance curve is tested by a micro-spectrophotometer, and no characteristic peaks of organic pollutants are found in the purified water. This shows that the porous polypyrrole solar evaporator has a good purification ability for organic pollutants.
[0060] 1.4 The purchased tomato plants with young fruits were taken out of the nutrient soil, their roots were washed with ultrapure water, and they were fixed in a plastic culture bottle containing Hoagland solution with a planting fence. The culture solution was changed every 2 to 3 days. After 7 days of adaptation, the tomatoes were divided into four groups: blank control group, nanoplastic group, purified water group, and purified residual water group. Among them, the treatment method of the nanoplastic group was to add green fluorescent PS-NPs to the Hoagland solution and make its concentration reach 50 mg·L -1 The treatment method for the purified water group and the residual water purification group was to add green fluorescent PS-NPs to the water to a concentration of 50 mg·L -1 After evaporation and purification by the porous polypyrrole system, the purified water and the remaining purified water in the beaker were collected and mixed with the Hoagland solution at a volume ratio of 1:1, and the adapted tomatoes were cultured in the solution. Three days later, the roots, stems, and fruits of the tomatoes were embedded in agar and sliced and observed using a confocal laser scanning microscope (CLSM). The results are as follows Fig.11 As shown, Fig.11a is a confocal microscopic image of tomato roots, stems, and fruit slices cultured in a culture solution prepared with purified water from nanoplastic wastewater. In it, it was found that the green fluorescence and red fluorescence intensities were similar and almost completely overlapped, indicating that what was observed was the autofluorescence of chloroplasts. The confocal images observed in the tomato roots, stems, and fruits cultured in the Hoagland solution prepared with the remaining purified water clearly showed that the green fluorescence intensity of some parts was significantly higher than that of the red fluorescence part ( Fig.11 b), through channel fusion, it is found that the enhanced green fluorescence part is nanoplastic. This also proves that the porous polypyrrole solar evaporator has the effect of purifying nanoplastic-contaminated water.
[0061] Transmission electron microscope photos of pure water, nanoplastic contaminated water in the nanoplastic group, purified water collected after evaporation purification by the porous polypyrrole system, and purified residual water in the beaker. Fig.12 As shown, from Fig.12 It can be seen that there is no nanoplastic in the purified water. This shows that the porous polypyrrole solar evaporator has a good purification ability for nanoplastics in water.
[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing porous polypyrrole, characterized in that: include: The pyrrole solution and the ferric chloride solution are mixed, heated for polymerization, and allowed to stand at room temperature after the reaction is completed to obtain porous polypyrrole.
2. The preparation method according to claim 1, characterized in that The concentration of the pyrrole solution is 0.8-1.2 mol / L, preferably 1 mol / L; Alternatively, the ferric chloride is ferric chloride hexahydrate; the concentration of the ferric chloride hexahydrate solution is 0.8-1.2 mol / L, preferably 1 mol / L.
3. The preparation method according to claim 1, characterized in that: The molar ratio of pyrrole to ferric chloride is 0.9 to 1.2:1, preferably 1:
1.
4. The preparation method according to claim 1, characterized in that: The temperature of the heating polymerization is 55 to 65° C., preferably 60° C.; the time of the heating polymerization is 0.5 to 1.5 h, preferably 1 h; Alternatively, the standing time at room temperature is 20 to 30 hours, preferably 24 hours.
5. The porous polypyrrole prepared by the preparation method according to any one of claims 1 to 4.
6. The porous polypyrrole according to claim 5, characterized in that The pore size of the porous polypyrrole is 3-40 μm.
7. A solar evaporator, characterized in that: The solar evaporator comprises the porous polypyrrole according to claim 5.
8. Use of the porous polypyrrole according to claim 5 and / or the solar evaporator according to claim 7 in water treatment.
9. The use according to claim 8, characterized in that The water treatment includes seawater evaporation and sewage treatment.
10. The use according to claim 9, characterized in that Wastewater treatment includes acid and alkali wastewater purification, organic dye wastewater purification and nano-plastic wastewater purification; Preferably, the organic dye comprises rhodamine b, Congo red and bromophenol blue.
Citation Information
Patent Citations
Preparation method of carbon nano tube reinforced conducting polymer hydrogel
CN105244189A
Preparation method of optothermal distillation membrane and efficient solar desalination device comprising optothermal distillation membrane
CN107829330A
Supramolecular hydrogel as well as preparation method and application thereof
CN113069594A
Bio-based photo-thermal microsphere as well as preparation method and application thereof
CN115991512A
Polypyrrole / diatomite-porous foam composite photo-thermal material as well as preparation method and application thereof
CN117924796A