Wear-resistant agent with repairing function as well as preparation method and application of wear-resistant agent

The wear-resistant agent prepared through the amidation reaction of modified thermoplastic acrylic resin and maleic anhydride-grafted polyethylene wax solves the problems of insufficient wax dispersion and scratch resistance in water-based inks and achieves high durability of water-based inks. Wear resistance and self-healing ability.

CN118725313APending Publication Date: 2024-10-01ZHONGSHAN FUREY PRINTING MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410959382.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The wax liquid added to water-based ink has poor dispersion in water and only has anti-friction properties but not scratch resistance, resulting in a high risk of scratches during application.

Method used

The amidation reaction product of modified thermoplastic acrylic resin and maleic anhydride-grafted polyethylene wax is used as a wear-resistant agent. Polyethylene wax, hydrophilic amino groups and hydroxyl groups are introduced into the molecular chain segments to form hydrogen bonds to improve dispersion. properties and self-healing capabilities, and fills pores in the coating to improve wear and scratch resistance.

Benefits of technology

Significantly improves the wear resistance and self-healing performance of water-based ink, forming a smoother and wear-resistant coating that can automatically recover after scratches and effectively repair large-area damage under thermal repair conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949847480000041
    Figure BDA0004949847480000041
  • Figure BDA0004949847480000042
    Figure BDA0004949847480000042
  • Figure BDA0004949847480000061
    Figure BDA0004949847480000061
Patent Text Reader

Abstract

The invention discloses a wear-resistant agent with a repairing function as well as a preparation method and application thereof, and belongs to the technical field of printing ink and manufacturing thereof. The wear-resistant agent with the repairing function provided by the invention is an amidation reaction product of modified thermoplastic acrylic resin and maleic anhydride grafted polyethylene wax; the modified thermoplastic acrylic resin is a polymerization product of an unsaturated amino compound and an acrylic monomer. The wear-resistant agent can effectively improve the wear resistance of the water-based ink, the dispersibility of the wear-resistant agent in water and the self-repairing performance of a coating formed by the water-based ink. The invention also provides a preparation method and application of the wear-resistant agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ink and its manufacturing technology, in particular to a wear-resistant agent with a repairing function and a preparation method and application thereof. Background Art

[0002] Water-based ink does not contain volatile organic solvents and is green and environmentally friendly. Water-based ink is a flowing substance with a certain viscosity formed by uniformly mixing components such as pigments, water-based binders, solvents and auxiliary additives. The main body of water-based ink is composed of pigments and water-based binders as dispersed phases and color phases. Among them, auxiliary additives usually include leveling agents and wear agents. The anti-friction additive is mainly a water-based wax emulsion, which improves the friction resistance of the ink by increasing the hardness of the ink film and reducing the friction coefficient. The mechanism of action is the low surface tension of the wax emulsion. Therefore, when added to the ink, it can rise to the surface of the ink by relying on its own low energy to form a spherical protective layer. After the ink dries, as the ink layer shrinks, the spherical spheres in the ink layer are closer to the spheres on the surface. Therefore, a wax layer is formed on the dried ink layer to resist friction.

[0003] However, there are certain limitations to adding wax to water-based inks. First, the dispersibility of wax in water is inferior to that in oily solvents. Second, although wax has anti-friction properties, it does not have scratch resistance. Therefore, even if anti-wear agents are added to water-based inks, there is still a high risk of scratches.

[0004] Therefore, if a wear-resistant agent with good dispersibility in water and scratch self-repair function can be prepared, it will greatly promote the application of water-based inks. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a wear-resistant agent with a repairing function, which can effectively improve the wear resistance of water-based ink, the dispersibility of the wear-resistant agent in water, and the self-repairing performance of the coating formed by the water-based ink.

[0006] The invention also provides a method for preparing the anti-wear agent.

[0007] The invention also provides application of the anti-wear agent.

[0008] According to an embodiment of the first aspect of the present invention, there is provided an anti-wear agent with a repairing function, wherein the anti-wear agent is an amidation reaction product of a modified thermoplastic acrylic resin and a maleic anhydride grafted polyethylene wax;

[0009] The modified thermoplastic acrylic resin is a polymerization product of an unsaturated amino compound and an acrylic acid monomer.

[0010] The anti-wear agent according to the embodiment of the present invention has at least the following beneficial effects:

[0011] (1) The molecular chain segment of the anti-wear agent contains polyethylene wax, so it has the initial anti-wear effect of the anti-wear agent.

[0012] (2) The molecular chain segments of the wear-resistant agent contain modified thermoplastic acrylic resin, which contains a large number of hydrophilic amino and hydroxyl groups, thereby improving the dispersibility of the wear-resistant agent in water.

[0013] (3) As mentioned above, the wear-resistant agent contains a large number of amino groups and hydroxyl groups, and a large number of hydrogen bonds can be formed between the two and within each of them. Under the action of hydrogen bonds, the wear-resistant agent has a certain elastic deformation, that is, it can automatically recover (self-repair) after a certain force is applied to the surface to produce scratches. Even if a small area of ​​rupture occurs, it can also be restored under the action of hydrogen bonds. That is, due to the introduction of the modified thermoplastic acrylic resin, the wear-resistant agent has a certain self-repairing ability.

[0014] (4) The coating formed by the acrylic resin is smoother and has better wear resistance and scratch resistance. The present invention introduces a modified thermoplastic acrylic resin into the wear-resistant agent to further improve its wear resistance and scratch resistance.

[0015] (5) In the water-based ink system, the wear-resistant agent is an auxiliary agent that fills the pores of the subject resin to a certain extent. The wear-resistant agent provided by the present invention has thermoplasticity as a whole, so if a large area of ​​the water-based ink coating is damaged, heat can be applied to the coating, so that the wear-resistant agent can change its shape according to the damaged shape and fill the pores to achieve the effect of repair.

[0016] According to some embodiments of the present invention, in the modified thermoplastic acrylic resin, the molar ratio of amino group to hydroxyl group is 1:10 to 20. For example, it can be 1:12 to 18. It can be about 1:15. This ratio limits the amount of hydrogen bonds to a certain extent. Within this range, the self-healing performance of the wear-resistant agent is good.

[0017] Furthermore, since amino is the main group that reacts with maleic anhydride grafted polyethylene wax, limiting this ratio limits the rotation (movement) range of the molecular chain in the wear-resistant agent to a certain extent. Within this range, the wear-resistant agent has suitable strength and thermoplasticity, and thus has good thermal repair performance.

[0018] Furthermore, in the present invention, the ratio is calculated according to the feed ratio, that is, the molar ratio of the amino group in the unsaturated amino compound to the hydroxyl group in the unsaturated amino compound and the acrylic acid monomer.

[0019] According to some embodiments of the present invention, the mass ratio of the modified thermoplastic acrylic resin to the maleic anhydride grafted polyethylene wax is 1:5 to 10, for example, 1:7 to 9, and more specifically, about 1:8.

[0020] According to an embodiment of the second aspect of the present invention, a method for preparing the anti-wear agent is provided, and the preparation method comprises the following steps:

[0021] S1. copolymerizing the acrylic monomer and the unsaturated amino monomer in the presence of an initiator to obtain the modified thermoplastic acrylic resin;

[0022] S2. subjecting the modified thermoplastic acrylic resin and the maleic anhydride grafted polyethylene wax to an amidation reaction to obtain the wear-resistant agent.

[0023] Since the preparation method adopts all the technical solutions of the wear-resistant agent of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.

[0024] According to some embodiments of the present invention, in step S1, the unsaturated amino monomer includes at least one of aminoacrylic acid, acrylamide, methacrylamide, N-hydroxymethyl acrylamide and sulfomethylated acrylamide.

[0025] According to some embodiments of the present invention, in step S1, the initiator includes at least one of ammonium persulfate, diisopropylbenzene oxide, tert-butyl peroxyhexanoate and azobisisobutyronitrile.

[0026] According to some embodiments of the present invention, in step S1, the ratio of the mass of the initiator to the mass sum of the acrylic acid monomer and the unsaturated amino monomer is 1:60-80. For example, it can be 1:65-75. More specifically, it can be about 1:70.

[0027] According to some embodiments of the present invention, in step S1, the copolymerization is carried out in a water medium, wherein the mass percentage of water in the copolymerization reaction system is 40-50%, for example, specifically 42-48%, and more specifically, about 45%.

[0028] According to some embodiments of the present invention, in step S1, the reaction temperature of the copolymerization is 80-90°C, for example, 82-88°C, and more specifically, about 85°C.

[0029] According to some embodiments of the present invention, in step S1, the copolymerization reaction time is 0.5 to 2 hours, for example, about 1 hour or about 1.5 hours.

[0030] According to some embodiments of the present invention, in step S2, the amidation reaction comprises the following steps performed sequentially:

[0031] S2a the maleic anhydride grafted polyethylene wax and condensation agent, activator mixed;

[0032] S2b. Mixing the mixture obtained in step S2a and the modified thermoplastic acrylic resin for reaction.

[0033] According to some embodiments of the present invention, in step S2a, the condensing agent includes 1-ethyl-(3-dimethylaminopropyl) carbodiimide salt (EDC.HCL for short).

[0034] According to some embodiments of the present invention, in step S2a, the activator is N-hydroxysuccinimide (NHS for short).

[0035] According to some embodiments of the present invention, in step S2a, the molar ratio of the condensing agent to the activating agent is 1:0.8-1.2, for example, specifically about 1:1.

[0036] According to some embodiments of the present invention, in step S2a, the mass ratio of the condensing agent to the maleic anhydride grafted polyethylene wax is 1:10 to 20. For example, it can be about 1:12, 1:15 or about 1:18.

[0037] According to some embodiments of the present invention, in step S2a, the mixing is performed in a water medium, wherein the mass percentage of water in the mixing system is 98-99.5%, for example, specifically about 99.2%.

[0038] According to some embodiments of the present invention, in step S2a, the mixing time is 5 to 15 minutes, for example, about 8 minutes, 10 minutes or about 12 minutes.

[0039] According to some embodiments of the present invention, in step S2b, the temperature of the mixing reaction is 40-60°C, for example, about 42°C, 45°C or about 48°C.

[0040] According to some embodiments of the present invention, in step S2b, the reaction time of the mixing reaction is 4 to 6 hours, for example, about 4.5 hours, 5 hours or about 5.5 hours.

[0041] According to some embodiments of the present invention, the preparation method further comprises a solvent removal after step S2. The end point of the solvent removal is that the obtained anti-wear agent is in an emulsion state with a solid content of 35-45%; the specific solid content may be about 40%. The solvent removal method comprises vacuum distillation. The temperature of the vacuum distillation is 70-90°C, specifically about 80°C. At this temperature, the molecular structure of the anti-wear agent will not be destroyed, and the solvent can be removed as quickly as possible.

[0042] According to an embodiment of the third aspect of the present invention, there is provided an aqueous ink, wherein the raw materials for preparing the aqueous ink include the abrasion resistant agent.

[0043] Since the water-based organic ink adopts all the technical solutions of the wear-resistant agent of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment, that is, the water-based ink has good wear resistance and repairability.

[0044] According to some embodiments of the present invention, the raw materials for preparing the water-based ink further include water-based acrylic resin, pigment, dispersant, defoamer, leveling agent and solvent water.

[0045] According to some embodiments of the present invention, the raw materials for preparing the water-based ink include, by weight:

[0046]

[0047] According to some embodiments of the present invention, the raw materials for preparing the water-based ink include, by weight:

[0048]

[0049] According to some embodiments of the present invention, the pigment includes at least one of titanium dioxide, phthalocyanine blue, benzidine yellow, permanent pink and carbon black.

[0050] According to some embodiments of the present invention, the dispersant comprises a SN-5029 type dispersant.

[0051] According to some embodiments of the present invention, the leveling agent includes at least one of ionic polyacrylate, polyether-modified siloxane, polyether-modified polydimethylsiloxane or acetylene glycol-based gemini surfactant.

[0052] According to some embodiments of the present invention, the defoaming agent includes at least one of polyether-modified polydimethylsiloxane, polyether-modified trisiloxane, polyether-siloxane copolymer containing fumed silica, polydimethylsiloxane, fluorosilicone and glycol siloxane.

[0053] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.

[0054] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values ​​2 and 3.

[0055] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION

[0056] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0057] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0058] Example 1

[0059] In this example, a wear-resistant agent with a repairing function is prepared, and the specific steps are as follows:

[0060] S1. Carry out the following reaction under the condition of isolating oxygen:

[0061] Adding acrylic acid monomer (CAS: 79-10-7) and acrylamide (CAS: 79-06-1) into water at a molar ratio of 15:1 to obtain a monomer solution, wherein the mass percentage of water is 45%;

[0062] Then, azobisisobutyronitrile (CAS: 78-67-1) was added to the monomer solution at a mass ratio of initiator azobisisobutyronitrile: (acrylic acid monomer + acrylamide) = 1:70;

[0063] Then, the mixture was stirred and polymerized at 85°C for 1 hour, and then the cover was opened to allow the reaction system to come into contact with air, thereby obtaining a modified thermoplastic acrylic resin.

[0064] S2. The modified thermoplastic acrylic resin obtained in step S1 and the maleic anhydride grafted polyethylene wax are subjected to amidation reaction at a mass ratio of 1:8 (based on solid mass) to obtain the anti-wear agent. The specific process is as follows:

[0065] S2a. Mix maleic anhydride grafted polyethylene wax (manufacturer: Honeywell, USA, model: A-C573P) with condensation agent EDC.HCL (CAS: 25952-53-8) and activator NHS (CAS: 6066-82-6) for 10 minutes; wherein the molar ratio of the activator to the condensation agent is 1:1; the mass ratio of the condensation agent to the maleic anhydride grafted polyethylene wax is 1:15; the mixing is carried out in water, and the mass percentage of water in the mixing system is 99%.

[0066] S2b. Mix the mixture obtained in step S2a and the modified thermoplastic acrylic resin obtained in step S1 for reaction, wherein the temperature of the mixing reaction is 50° C. and the duration is 5 hours.

[0067] S3. The mixture obtained in step S2 was distilled under reduced pressure at 75°C until the solid content of the obtained emulsion reached 40%.

[0068] Example 2

[0069] This example prepares a wear-resistant agent with a repairing function. The specific steps are different from those in Example 1 in that:

[0070] In step S1, acrylamide is replaced by N-[tris(hydroxymethyl)methyl]acrylamide (CAS: 13880-05-2), and the molar ratio of acrylic acid monomer to N-[tris(hydroxymethyl)methyl]acrylamide is 12:1 (the ratio of hydroxyl groups to amino groups is the same as that in Example 1).

[0071] Comparative Example 1

[0072] This example prepares an anti-wear agent, which is different from Example 1 in that:

[0073] In step S1, the monomer does not include acrylamide.

[0074] Application Examples

[0075] This example provides a water-based ink, the specific ingredients are as follows:

[0076]

[0077] Test Case

[0078] In the first aspect of this example, the dispersibility of the anti-wear agent obtained in the embodiment and the comparative example was tested by visual inspection to see whether it was uniform and whether it was demulsified after standing for 24 hours.

[0079] The second aspect of this example tests the wear resistance of the coating formed by the water-based ink obtained in the application example. The test method is: use the SUTHERLAND2000 printing friction tester to perform the same friction treatment on the printed samples (85rpm, 21b counterweight, 50 times of friction). The wear resistance of the coating is evaluated by the density decay rate. The smaller the density decay rate, the better the abrasion resistance. The density decay rate R is characterized as follows: R = (D0–D g ) / D0×100%; where D0 is the density of the printed pattern before friction, D g is the density of the printed pattern after friction. The density attenuation rate is characterized by the average value of the test results of 5 sample strips. The pattern printing condition is to use IGT-F1 printability tester for proofing. The printing pressure is 150N, the anilox roller pressure is 250N, the printing speed is 0.3m / s, and the anilox roller screen number used is 200dpi.

[0080] The fourth aspect of this example tests the repair ability of the coating formed by the water-based ink obtained in the application example, wherein the test method used for the self-repair performance is: using a ZBQ four-sided coating preparation device (Pushen Testing Instruments (Shanghai) Co., Ltd.) to ensure that the overall thickness of the prepared coating is 60 μm, and the test is carried out in a LT-TH-80 constant temperature and humidity chamber (Dongguan Lituo Testing Instruments Co., Ltd.). When performing the scratch test, a Flying Eagle 74-C single-sided security blade (Shanghai Gillette Co., Ltd.) is used to produce a scratch with a depth of 60 μm on the self-repairing coating, so that the coating is just scratched. OM is used to observe the repair changes when the coating scratch is generated and after standing in a constant temperature and humidity chamber (temperature of 25°C and humidity of 45%) for 3 days, and the self-repair performance is specifically characterized by the scratch width change rate. The test method for thermal repair performance is to characterize it by the scratch width change rate after being stored in a constant temperature and humidity chamber (temperature of 110°C and humidity of 45%) for 6 hours. The test of the repair performance is repeated 4 times, and the average value is taken after removing significant outliers.

[0081] The results of the above tests are shown in Table 1.

[0082] Table 1 Performance test results of embodiments, comparative examples and controls

[0083] Example 1 Example 2 Comparative Example 1 Comparison 1 Comparison 2 Dispersibility Uniform Uniform Slight demulsification Uniform Layering Wear resistance % 4.1 5.6 14.9 17.1 8.6 Self-repair % 33.87 32.70 12.92 17.85 11.62 Hotfix % 86.25 86.39 62.38 59.79 77.61

[0084] According to the above results, the wear-resistant agent provided by the present invention has good water dispersibility, and the water-based ink containing the wear-resistant agent has excellent wear resistance and repair performance.

[0085] By comparing Example 1 and Example 2, it can be seen that if the amount of unsaturated amino monomer is reduced within the scope provided by the present invention, it is equivalent to reducing the number of bonds between the modified thermoplastic acrylic resin and the maleic anhydride grafted polyethylene wax. Therefore, during the friction process, the coating surface including the wear-resistant agent will deform, etc., which reduces the density of the printed pattern, that is, the wear resistance is reduced to a certain extent; at the same time, due to the decrease in the amino content, the hydroxyl content in the coating decreases, which reduces the self-repair ability to a certain extent; but at the same time, the molecular chain of the wear-resistant agent is more likely to move and deform under the action of heat, so the thermal repair performance is slightly improved.

[0086] In Comparative Example 1, the thermoplastic acrylic resin does not include amino groups, so the obtained wear-resistant agent is actually a mixture of thermoplastic acrylic resin and maleic anhydride grafted polyethylene wax. Therefore, the wear-resistant agent obtained in Comparative Example 1 exhibits stratification after standing for 2 days.

[0087] By comparing Example 1 with Comparative Example 1 and Controls 1 to 2, it can be seen that in the wear-resistant agent provided by the present invention, a chemical reaction occurs between the modified thermoplastic acrylic resin and the maleic anhydride grafted polyethylene wax, resulting in a synergistic effect, which can significantly improve the wear resistance and repair performance compared with a single or mixed one.

[0088] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A wear-resistant agent with a repairing function, characterized in that: The anti-wear agent is an amidation reaction product of a modified thermoplastic acrylic resin and maleic anhydride grafted polyethylene wax; The modified thermoplastic acrylic resin is a polymerization product of an unsaturated amino compound and an acrylic acid monomer.

2. The wear-resistant agent according to claim 1, characterized in that The mass ratio of the modified thermoplastic acrylic resin to the maleic anhydride grafted polyethylene wax is 1:5-10.

3. The wear-resistant agent according to claim 1, characterized in that In the modified thermoplastic acrylic resin, the molar ratio of amino group to hydroxyl group is 1:10-20.

4. A method for preparing the anti-wear agent according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: S1. copolymerizing the acrylic monomer and the unsaturated amino monomer in the presence of an initiator to obtain the modified thermoplastic acrylic resin; S2. subjecting the modified thermoplastic acrylic resin and the maleic anhydride grafted polyethylene wax to an amidation reaction to obtain the wear-resistant agent.

5. The preparation method according to claim 4, characterized in that: In step S1, the unsaturated amino monomer includes at least one of aminoacrylic acid, acrylamide, methacrylamide, N-hydroxymethyl acrylamide and sulfomethylated acrylamide.

6. The preparation method according to claim 4, characterized in that: In step S2, the amidation reaction comprises the following steps performed in sequence: S2a the maleic anhydride grafted polyethylene wax and condensation agent, activator mixed; S2b. Mixing the mixture obtained in step S2a and the modified thermoplastic acrylic resin for reaction.

7. The preparation method according to claim 6, characterized in that: In step S2a, the condensing agent includes 1-ethyl-(3-dimethylaminopropyl)carbodiimide salt; and / or, in step S2a, the activating agent is N-hydroxysuccinimide NHS.

8. The preparation method according to claim 7, characterized in that: In step S2a, the molar ratio of the condensing agent to the activating agent is 1:0.8-1.2; and / or, in step S2a, the mass ratio of the condensing agent to the maleic anhydride grafted polyethylene wax is 1:10-20.

9. The preparation method according to claim 6, characterized in that: In step S2b, the temperature of the mixed reaction is 40-60°C; and / or, in step S2b, the reaction time of the mixed reaction is 4-6h.

10. A water-based ink, characterized in that: The raw materials for preparing the water-based ink include the wear-resistant agent as described in any one of claims 1 to 3.