Photochromic luminescent crystal material for extremely sensitively detecting water-phase Hg < 2 + > and preparation method of photochromic luminescent crystal material
By preparing a three-dimensional photochromic luminescent crystal material [Cd(L)(OBA)]n, the problem of insufficient Hg2+ detection sensitivity in the prior art was solved, and high-sensitivity Hg2+ detection in aqueous phase was achieved, which is suitable for environmental detection.
Patent Information
- Application Number
- CN202410691258.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-30
AI Technical Summary
Existing organic photochromic molecular materials lack sufficient sensitivity in detecting Hg2+, making it difficult to meet the needs of scientific and technological development and environmental monitoring.
A three-dimensional photochromic luminescent crystal material [Cd(L)(OBA)]n was prepared by reacting cadmium acetate dihydrate, 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene, and 4,4-diphenyl ether dicarboxylic acid in a mixed solvent in a specific ratio to form a highly sensitive photochromic luminescent crystal for the detection of Hg2+ in aqueous phase.
It achieves extremely sensitive detection of Hg2+ in aqueous phase, with a luminescence quenching constant as high as 8.31×104M-1 and a detection limit as low as 7.62×10-7M. It is simple, reliable and suitable for industrial applications.
Smart Images

Figure CN118725318A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photochromic luminescence detection functional materials, and specifically relates to a method for extremely sensitively detecting Hg in water phase. 2+ Photochromic luminescent crystal material and preparation method thereof. Background Art
[0002] Divalent mercury ion (Hg 2+ ) is one of the most important and deadly heavy metal ions. Hg 2+ It is widely used in industry. Due to industrial emissions, Hg 2+ It is easily accumulated in water, air and soil in the daily environment. Hg 2+ With terrible toxicity, it poses a great threat to the environment and public health. Among them, mercury can damage organs such as the brain, heart, and kidneys. Even at low concentrations, the accumulation of mercury can cause serious damage to the human body.
[0003] Luminescent metal-organic framework detection materials have the advantages of convenient, rapid, sensitive and highly selective detection, and have been developed and applied in the field of luminescence detection. Organic ligands play a decisive role in the luminescence detection performance of metal-organic framework crystal materials.
[0004] In recent years, organic photochromic molecules have been widely studied and applied in biological probes, cell imaging, anti-counterfeiting materials, etc. However, organic photochromic molecular materials often cannot meet the development of science and technology and people's growing material needs. Therefore, it is of great significance to develop organic photochromic molecules into functional organic ligands to construct metal-organic framework crystal materials with luminescence detection function. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a photochromic luminescent crystal material, comprising:
[0008] The photochromic luminescent crystal material is a three-dimensional structure, and its unit cell parameters are: α=90°,β=90°,γ=90°,the unit cell volume is Z = 8;
[0009] The chemical formula is [Cd(L)(OBA)] n , wherein L represents 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene, OBA represents 4,4-diphenyl ether dicarboxylic acid, and n is an arbitrary value.
[0010] Another object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a photochromic luminescent crystal material.
[0011] In order to solve the above technical problems, the present invention provides the following technical solutions: comprising:
[0012] Cadmium acetate dihydrate, 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene, and 4,4-diphenyl ether dicarboxylic acid are added to a mixed solvent of water and ethanol and stirred to prepare a mixed solution;
[0013] The mixed solution is placed in a sealed reactor and heated to react, then slowly cooled to room temperature. The product is filtered, washed, and dried to obtain a photochromic luminescent crystal material [Cd(L)(OBA)] n ;
[0014] As a preferred scheme for the preparation method of the photochromic luminescent crystal material of the present invention, the molar ratio of cadmium acetate dihydrate, 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene and 4,4-diphenyl ether dicarboxylic acid is 1:0.25~0.75:0.5~1.5.
[0015] As a preferred solution of the method for preparing the photochromic luminescent crystal material of the present invention, the volume ratio of water to ethanol in the mixed solvent is 1:0.5-2.
[0016] As a preferred solution of the method for preparing the photochromic luminescent crystal material of the present invention, the volume of the mixed solvent of water and ethanol required for each 0.1 mmol of cadmium acetate dihydrate is 3 to 12 ml.
[0017] As a preferred embodiment of the method for preparing the photochromic luminescent crystal material of the present invention, the heating reaction has a heating temperature of 100 to 180° C. and a heating time of 48 to 84 hours.
[0018] As a preferred solution of the method for preparing the photochromic luminescent crystal material of the present invention, the temperature is lowered to room temperature, wherein the cooling rate is 2-5°C / h.
[0019] Another object of the present invention is to overcome the deficiencies in the prior art and provide a photochromic luminescent crystal material for detecting Hg in water phase. 2+ Application in.
[0020] As the photochromic luminescent crystal material of the present invention, it is useful for detecting Hg in water phase 2+ A preferred embodiment of the application of the invention, wherein: the photochromic luminescent crystal material photochromizes and then quenches the light to detect Hg in water phase 2+ The quenching constant is 8.31×10 4 M -1 .
[0021] As the photochromic luminescent crystal material of the present invention, it is useful for detecting Hg in water phase 2+ A preferred embodiment of the application of the invention, wherein: the photochromic luminescent crystal material photochromizes and then quenches the light to detect Hg in water phase 2+ The detection limit is 7.62×10 -7 M.
[0022] Beneficial effects of the present invention:
[0023] The present invention synthesizes a photochromic luminescent crystal material [Cd(L)(OBA)] based on 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene photochromic functional organic ligand for the first time. n The synthesis method is extremely simple, the route is mild and easy to control, and the obtained material [Cd(L)(OBA)] n Can be used to detect Hg in water phase 2+ Compared with the existing technology, the use of this crystal material for detection is simple and reliable, and the detection of Hg in water phase is carried out by luminescence quenching after photochromism. 2+ The quenching constant is as high as 8.31×10 4 M -1 , the detection limit is as low as 7.62×10 -7 M, is currently the most sensitive detection of Hg 2+ The photochromic luminescent crystal material has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0025] Figure 1 The crystalline material [Cd(L)(OBA)] prepared in Example 1 of the present invention n The three-dimensional crystal structure of .
[0026] Figure 2 The crystalline material [Cd(L)(OBA)] prepared in Example 1 of the present inventionn Powder X-ray diffraction spectrum.
[0027] Figure 3 The crystalline material [Cd(L)(OBA)] prepared in Example 1 of the present invention n Excitation and emission spectra of the aqueous suspension (0.1 mg / mL) before color change.
[0028] Figure 4 The crystalline material [Cd(L)(OBA)] prepared in Example 1 of the present invention n Excitation and emission spectra of the aqueous suspension (0.1 mg / mL) after color change.
[0029] Figure 5 The luminescent crystal material [Cd(L)(OBA)] prepared in Example 1 of the present invention n The luminescence intensity change curve of adding different volumes of divalent mercury ion aqueous solution (1mmol / L) into the water suspension.
[0030] Figure 6 The crystalline material [Cd(L)(OBA)] prepared in Example 1 of the present invention n Quenching constant curve for detection of divalent mercuric ions.
[0031] Figure 7 The crystalline material [Cd(L)(OBA)] prepared in Example 1 of the present invention n Detection limit curve for detecting divalent mercuric ions.
[0032] Figure 8 The luminescent crystal material [Cd(L)(OBA)] prepared in Comparative Example 1 of the present invention to Example 1 of the present invention n Graph showing the quenching efficiency when different cations are added to the aqueous suspension. DETAILED DESCRIPTION
[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0034] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0035] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0036] Unless otherwise specified, the chemical reagents used in the examples of the present invention are all commercially available analytically pure.
[0037] The calculation method of the yield in the embodiment of the present invention is: the yield is calculated based on L, and the calculation steps are:
[0038] m(actual crystal) / m(L complete reaction)
[0039] Example 1
[0040] This embodiment provides a method for preparing a photochromic luminescent crystal material, which is specifically as follows:
[0041] 1) 0.1 mmol of cadmium acetate dihydrate, 0.05 mmol of 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene, and 0.1 mmol of 4,4-diphenyl ether dicarboxylic acid were added into 6 mL of a mixed solvent (V water: V ethanol = 1:1) and stirred to prepare a mixed solution;
[0042] 2) The obtained mixed solution was placed in a sealed reactor and heated to 140°C for 72 hours. The temperature was slowly cooled to room temperature at a rate of 5°C / h. The product was filtered, washed with deionized water and ethanol, and dried in vacuo at 80°C for 30 minutes to obtain a crystalline material [Cd(L)(OBA)] n , the calculated yield is: 38.4%.
[0043] The single crystal structure of the crystalline material of the present invention was determined using a Bruker D8 VENTURE X-ray single crystal diffractometer. The specific crystal structure determination data are shown in Table 1.
[0044] Table 1 Crystal structure determination data
[0045]
[0046]
[0047] Figure 1 This is a three-dimensional crystal structure diagram of the crystalline material [Cd(L)(OBA)]n prepared in this example.
[0048] Figure 2 The crystalline material prepared in this example [Cd(L)(OBA)] n Powder X-ray diffraction spectrum, as can be seen from Table 1, its unit cell parameters are: α=90°,β=90°,γ=90°,the unit cell volume is Z=8.
[0049] Figure 3 , Figure 4 The crystalline material prepared in this example [Cd(L)(OBA)] n Excitation and emission spectra of aqueous suspension (0.1 mg / mL) before and after color change; Crystal material [Cd(L)(OBA)] n After photochromism, the excitation and emission spectra are obviously red-shifted.
[0050] Application Testing
[0051] Figure 5 To 2mL, the concentration of 0.1mg / mL crystalline material [Cd(L)(OBA)] n Different volumes of Hg at a concentration of 1 mmol / L were added to the aqueous suspension. 2+ The luminescence intensity change curve of aqueous solution shows that as Hg 2+ As the amount of ions increases gradually, the luminescence intensity of the suspension gradually quenches.
[0052] Figure 6 , Figure 7 They are respectively the photochromic crystal materials of the present invention [Cd(L)(OBA)] n Detection of Hg in water phase 2+ The quenching constant curve and detection limit curve of the material were obtained. The results showed that the quenching constant of the photochromic material for the detection of metronidazole in water phase was as high as 8.31×10 4 M -1 , the detection limit is as low as 7.62×10 -7 M, indicating that the detection material provided by the present invention can detect Hg in water phase with high sensitivity 2+ .
[0053] Comparative Example 1
[0054] To the luminescent crystal material [Cd(L)(OBA)] prepared in Example 1 n The same concentration and volume of different cations (Na + , K + Mg 2+ 、Al 3+ 、Ag + 、Cd 2+ 、Zn 2+ Cr 3+ , Hg 2+ ), detect its quenching efficiency, and obtain a quenching efficiency comparison chart, such as Figure 8 As shown. It can be seen that only Hg2+ The luminescent crystal material [Cd(L)(OBA)] prepared by the present invention can be n Obvious emission quenching occurs, that is, [Cd(L)(OBA)] obtained in this application n Hg 2+ It has specific detection effect.
[0055] Example 2
[0056] The difference between this embodiment and embodiment 1 is that the molar mass of 4,4-diphenyl ether dicarboxylic acid is adjusted to 0.025 mmol, and the rest of the preparation process is the same as that of embodiment 1, to obtain the photochromic luminescent crystal material [Cd(L)(OBA)] of this embodiment. n , the calculated yield is: 26.9%.
[0057] Example 3
[0058] The difference between this embodiment and embodiment 1 is that the molar mass of 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene is adjusted to 0.075 mmol, and the rest of the preparation process is the same as that of embodiment 1 to obtain the photochromic luminescent crystal material [Cd(L)(OBA)] of this embodiment. n , the calculated yield is: 35.3%.
[0059] Comparative Example 2
[0060] The difference between this comparative example and Example 1 is that the molar ratio of cadmium acetate dihydrate, 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene, and 4,4-diphenyl ether dicarboxylic acid is adjusted to 1:1:1, and the rest of the preparation process is the same as Example 1. The solution is clear, no crystals are generated, and the preparation is unsuccessful.
[0061] Table 2 shows the synthesis conditions of Examples 1 to 3 and Comparative Example 2 and the yields under the corresponding conditions.
[0062] Table 2
[0063]
[0064] It can be seen from Table 2 that the yield of the synthesized product is related to the molar ratio of the organic complex and 4,4-diphenylether dicarboxylic acid. When the molar ratio is 1:1, the photochromic luminescent crystal material cannot be successfully synthesized.
[0065] Example 4
[0066] The difference between this embodiment and embodiment 1 is that the cooling rate is adjusted to 2°C / h, and the rest of the preparation process is the same as that of embodiment 1, and the photochromic luminescent crystal material [Cd(L)(OBA)] of this embodiment is obtained. n, the calculated yield is: 36.2%.
[0067] Comparative Example 3
[0068] The difference between this comparative example and Example 1 is that the cooling rate is adjusted to 1°C / h, and the rest of the preparation process is the same as Example 1. The yield is not significantly improved, the experimental process is slow, and unnecessary waste of resources occurs.
[0069] Comparative Example 4
[0070] The difference between this comparative example and Example 1 is that the cooling rate is adjusted to 6°C / h, and the rest of the preparation process is the same as Example 1. This affects the crystallization of the crystal, and the quality is poor, so subsequent tests cannot be performed.
[0071] Table 3 shows the synthesis conditions of Example 1, Example 4 and Comparative Example 3 and Comparative Example 4 and the yields under the corresponding conditions.
[0072] Table 3
[0073]
[0074] It can be seen from Table 3 that the yield of the synthesized product is related to the cooling rate. When the cooling rate is 2-5°C / h, the preparation can be successful, while when the cooling rate is too high or too low, the photochromic luminescent crystal material cannot be synthesized well.
[0075] Example 5
[0076] The difference between this embodiment and embodiment 1 is that the volume of the mixed solvent is adjusted to 9 mL (V water: V ethanol = 1:1), and the rest of the preparation process is the same as that of embodiment 1, to obtain the photochromic luminescent crystal material [Cd(L)(OBA)] of this embodiment. n , the calculated yield is: 28.5%.
[0077] Comparative Example 5
[0078] The difference between this comparative example and Example 1 is that the volume of the mixed solvent is adjusted to 2 mL (V water: V ethanol = 1:1), and the rest of the preparation process is the same as Example 1. Unable to prepare successfully.
[0079] Comparative Example 6
[0080] The difference between this comparative example and Example 1 is that the volume of the mixed solvent is adjusted to 13 mL (V water: V ethanol = 1:1), and the rest of the preparation process is the same as Example 1. Unable to prepare successfully.
[0081] Table 4 shows the synthesis conditions of Example 1, Example 5, Comparative Example 5 and Comparative Example 6 and the yields under the corresponding conditions.
[0082] Table 4
[0083]
[0084] It can be seen from Table 4 that the yield of the synthesized product is related to the volume of the mixed solvent. If the volume of the mixed solvent is too high or too low, the photochromic luminescent crystal material cannot be successfully synthesized.
[0085] Example 6
[0086] The difference between this embodiment and embodiment 1 is that the reaction temperature is adjusted to 100° C., and the rest of the preparation process is the same as that of embodiment 1, to obtain the photochromic luminescent crystal material [Cd(L)(OBA)] of this embodiment. n , the calculated yield is: 5.4%.
[0087] Example 7
[0088] The difference between this embodiment and embodiment 1 is that the reaction temperature is adjusted to 180°C, and the rest of the preparation process is the same as that of embodiment 1, and the photochromic luminescent crystal material [Cd(L)(OBA)] of this embodiment is obtained. n , the calculated yield is: 17.3%.
[0089] Comparative Example 7
[0090] The difference between this comparative example and Example 1 is that the reaction temperature is adjusted to 190° C., and the rest of the preparation process is the same as Example 1. Unable to prepare successfully.
[0091] Table 5 shows the synthesis conditions of Example 1, Example 6, Example 7 and Comparative Example 7 and the yields under the corresponding conditions.
[0092] Table 5
[0093]
[0094]
[0095] It can be seen from Table 5 that the yield of the synthesized product is related to the heating temperature. If the heating temperature is too high, the photochromic luminescent crystal material cannot be successfully synthesized.
[0096] Example 8
[0097] The difference between this embodiment and embodiment 1 is that the volume ratio of water to ethanol in the mixed solvent is adjusted to 1:0.5, and the rest of the preparation process is the same as that of embodiment 1, to obtain the photochromic luminescent crystal material [Cd(L)(OBA)] of this embodiment. n , the calculated yield is: 13.2%.
[0098] Example 9
[0099] The difference between this embodiment and embodiment 1 is that the volume ratio of water to ethanol in the mixed solvent is adjusted to 1:2, and the rest of the preparation process is the same as that of embodiment 1, to obtain the photochromic luminescent crystal material [Cd(L)(OBA)] of this embodiment. n , the calculated yield is: 15.6%.
[0100] Comparative Example 8
[0101] The difference between this comparative example and Example 1 is that the volume ratio of water to ethanol in the mixed solvent is adjusted to 1:3, and the rest of the preparation process is the same as Example 1. The solution is clear, no crystal is generated, and the preparation is unsuccessful.
[0102] Comparative Example 9
[0103] The difference between this comparative example and Example 1 is that ethanol is not added to the mixed solvent, and the rest of the preparation process is the same as Example 1. The solution is turbid, with a large amount of precipitation, and no crystals are generated, and the preparation is unsuccessful.
[0104] Table 6 shows the synthesis conditions of Example 1, Example 8, Example 9 and Comparative Example 8, Comparative Example 9 and the yields under the corresponding conditions.
[0105] Table 6
[0106]
[0107]
[0108] It can be seen from Table 6 that the yield of the synthesized product is related to the volume ratio of water to ethanol in the mixed solvent. If the volume ratio of water to ethanol in the mixed solvent is too large or too small, the photochromic luminescent crystal material cannot be successfully synthesized.
[0109] Comparative Example 10
[0110] The difference between this comparative example and Example 1 is that cadmium acetate dihydrate is changed to cadmium nitrate tetrahydrate, and the rest of the preparation process is the same as that of Example 1. The solution is turbid, with a large amount of precipitation, and no crystals are generated, and the preparation is unsuccessful.
[0111] Comparative Example 11
[0112] The difference between this comparative example and Example 1 is that cadmium acetate dihydrate is changed to cadmium chloride pentahydrate, and the rest of the preparation process is the same as that of Example 1. The solution is turbid, with a large amount of precipitation, and no crystals are generated, and the preparation is unsuccessful.
[0113] In summary, the present invention provides a highly sensitive method for detecting Hg in water based on 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene photochromic functional organic ligand. 2+The preparation method and product of the photochromic luminescent crystal material have a simple and easy-to-control synthesis route, and the product yield can reach 38.4%, which is suitable for industrial production and promotion. Compared with the existing technology, the use of the crystal material for detection is simple and reliable, and the luminescence quenching detection of Hg in water phase is 2+ The quenching constant is as high as 8.31×10 4 M -1 , the detection limit is as low as 7.62×10 -7 M, is currently the most sensitive detection of Hg 2+ The luminescent crystal material has broad application prospects.
[0114] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A photochromic luminescent crystal material, Features: include, The photochromic luminescent crystal material is a three-dimensional structure, and its unit cell parameters are: α=90°,β=90°,γ=90°,the unit cell volume is Z = 8; The chemical formula is [Cd(L)(OBA)] n , wherein L represents 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene, OBA represents 4,4-diphenyl ether dicarboxylic acid, and n is an arbitrary value.
2. The method for preparing the photochromic luminescent crystal material according to claim 1, Features: include, Cadmium acetate dihydrate, 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene, and 4,4-diphenyl ether dicarboxylic acid are added to a mixed solvent of water and ethanol and stirred to prepare a mixed solution; The mixed solution is placed in a sealed reactor and heated to react, then slowly cooled to room temperature. The product is filtered, washed, and dried to obtain a photochromic luminescent crystal material [Cd(L)(OBA)] n .
3. The method for preparing the photochromic luminescent crystal material according to claim 2, Features: The molar ratio of the cadmium acetate dihydrate, 9,10-bis(di(pyrimidin-5-yl)methylene)-9,10-dihydroanthracene and 4,4-diphenyl ether dicarboxylic acid is 1:0.25-0.75:0.5-1.
5.
4. The method for preparing the photochromic luminescent crystal material according to claim 2, Features: The volume ratio of water to ethanol in the mixed solvent is 1:0.5-2.
5. The method for preparing the photochromic luminescent crystal material according to claim 3, Features: The volume of the water and ethanol mixed solvent required for each 0.1 mmol of cadmium acetate dihydrate is 3 to 12 mL.
6. The method for preparing the photochromic luminescent crystal material according to claim 2, Features: The heating reaction, wherein the heating temperature is 100-180° C., and the heating time is 48-84 hours.
7. The method for preparing the photochromic luminescent crystal material according to claim 2, Features: The temperature is lowered to room temperature, wherein the cooling rate is 2-5°C / h.
8. The photochromic luminescent crystal material prepared by the preparation method according to any one of claims 2 to 7 is used to detect Hg in water phase 2+ Application in.
9. The photochromic luminescent crystal material as claimed in claim 8 is used to detect Hg in water phase 2+ Applications in Features: The photochromic luminescent crystal material detects Hg in water phase by luminescence quenching after photochromism 2+ The quenching constant is 8.31×10 4 M -1 .
10. The photochromic luminescent crystal material as claimed in claim 8 is used to detect Hg in water phase 2+ Applications in Features: The photochromic luminescent crystal material detects Hg in water phase by luminescence quenching after photochromism 2+ The detection limit is 7.62×10 -7 M.
Citation Information
Patent Citations
Preparation method and application of luminescent crystal material for extremely sensitive aqueous phase detection of permanganate
CN113845534A
Zinc coordination polymer based on organic ligand with photochromic function as well as preparation method and application of zinc coordination polymer
CN116444814A
Luminescent crystal material for extremely sensitively detecting aqueous-phase Fe < 3 + > and preparation method thereof
CN117603462A
Organic layer comprising regions having different electronic properties
WO2024042491A1