Preparation method and application of functional group modified titanium-based metal organic framework material MIP-207
The MIP-207 catalyst, a titanium-based metal organic framework material modified with functional groups, solves the shortcomings of hydrodesulfurization and oxidative desulfurization technologies in the existing technology, achieves efficient deep desulfurization and good cycle performance at room temperature, and improves catalytic oxidation fuel desulfurization. effect.
Patent Information
- Application Number
- CN202410746071.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-11
AI Technical Summary
The existing hydrodesulfurization technology has harsh conditions and is difficult to effectively remove thiophene sulfides in oil products. The quality of the oil products has declined, and the catalytic effect of the oxidative desulfurization technology catalyst is limited.
The MIP-207 catalyst, a titanium-based metal-organic framework material modified with functional groups, was synthesized through the reflux method and applied to catalyze oxidation fuel desulfurization at room temperature. The rich Ti-Ox clusters and different functional groups were used to improve the catalytic efficiency.
Achieve deep fuel oxidation desulfurization (sulfur content less than 3ppm) at room temperature, and significantly improve the catalytic efficiency and recycling performance of the catalyst.
Smart Images

Figure CN118725320A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel catalysts, and specifically relates to a preparation method of a functional group-modified titanium-based metal organic framework material MIP-207 and its application in catalytic oxidation desulfurization of fuel at room temperature. Background Art
[0002] During the combustion of fuel, sulfur oxides (SOx) are released. These SOx enter the atmosphere with the exhaust gas of automobiles, causing a series of environmental problems such as haze and acid rain. Therefore, countries and regions around the world have legislated to limit the concentration of sulfides in oil products, and the standards are becoming increasingly strict. At present, hydrodesulfurization technology (HDS) is often used in industry to remove sulfides from oil products. However, the reaction conditions of hydrodesulfurization are harsh. If deep desulfurization is to be achieved, high temperature and pressure are required, a large amount of hydrogen is consumed, and the quality of oil products will be reduced. In order to make up for the disadvantage that hydrodesulfurization technology is difficult to remove thiophene sulfides in oil products, oxidative desulfurization technology can be used. Oxidative desulfurization technology refers to the use of an oxidant to oxidize thiophene sulfides to their corresponding thiophene sulfones under the catalysis of a catalyst, thereby separating the highly polar sulfone sulfides from non-polar oil products and achieving the removal of sulfides from oil products. The catalytic effect of the catalyst plays an important role in oxidative desulfurization.
[0003] Metal-organic framework materials (MOFs) are organic-inorganic hybrid materials formed by self-assembly of metal ions or clusters and organic ligands. MIP-207, as a newly emerging titanium-based metal-organic framework (Ti-MOFs) material, has the characteristics of large specific surface area, high porosity, rich metal active sites, and diverse structures. Since only two of the three carboxyl groups in the 1,3,5-benzenetricarboxylic acid (BTC) ligand of MIP-207 participate in coordination, the other carboxylic acid does not participate in coordination and can be replaced by other functional groups. Therefore, MIP-207 can be modified by introducing different functional groups. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a preparation method and application of a functional group-modified MIP-207 catalyst. The present invention uses isopropyl titanate as a titanium source, an initial ligand 1,3,5-benzenetricarboxylic acid (BTC) and a functional group-modified ligand as an organic framework, and adopts a reflux method to synthesize a novel functional group-modified titanium-based metal organic framework material MIP-207.
[0005] The preparation method of the functional group modified titanium-based metal organic framework material MIP-207 comprises the following steps:
[0006] Add acetic acid and acetic anhydride into a round-bottom flask and stir thoroughly. Then, add isopropyl titanate as a titanium source to the mixed solution, and then add x mmol of a functional group-modified ligand and (10-x) mmol of an initial ligand BTC. After being stirred thoroughly, reflux the mixed solution for reaction. After the reaction is completed, separate the solid powder in the mixed solution by centrifugation, and finally wash, activate, and vacuum dry the solid.
[0007] Furthermore, the dosage of isopropyl titanate, functional group modified ligand, initial ligand BTC, acetic acid and acetic anhydride is 6.75mmol:xmmol:(10-x)mmol:25mL:25mL; wherein x is 2.5-5; that is, the functional group modified ligand accounts for 25%-50% of the total ligand molar amount.
[0008] Furthermore, the temperature of the reflux reaction is 120° C., and the time is 10 to 14 hours.
[0009] Furthermore, the washing and activation operation is: washing with boiling acetone three times.
[0010] Furthermore, the vacuum drying temperature is 40-55°C.
[0011] The structural formula of the initial ligand 1,3,5-benzenetricarboxylic acid is:
[0012]
[0013] The functional group-modified ligand is 5-aminoisophthalic acid, 5-nitrobenzeneisophthalic acid, 5-hydroxyisophthalic acid or isophthalic acid; the structural formula is:
[0014]
[0015] -R: -NH2, -NO2, -OH or -H;
[0016] The functional group modified titanium-based metal organic framework material MIP-207 prepared by the present invention is used in catalytic oxidation fuel desulfurization. The specific application method is:
[0017] Add model oil and extractant to the double-necked jacketed reaction bottle, add functional group-modified titanium-based metal organic framework material MIP-207 as a catalyst, place it on a magnetic stirrer, install a condenser above the reaction bottle, and pass the reaction bottle into a water bath. Use a microinjection needle to add the oxidant H2O2 to the reaction bottle to start the reaction. During the reaction, take out the upper oil phase at the same time to detect the sulfur content in the oil. Set up 4 groups of parallel experiments with the above experimental device to test the catalytic oxidation desulfurization performance of MIP-207 modified with each functional group.
[0018] The ratio of the model oil, the extractant and the catalyst is 5 mL: 1-5 mL: 25-75 mg; the temperature of the water bath is 20-50° C.;
[0019] Preferably, the usage ratio of the model oil, the extractant and the catalyst is 5 mL:1 mL:50 mg; and the temperature of the water bath is 25°C.
[0020] Wherein, the oxygen-sulfur ratio of the reaction is 2 to 5, preferably 3;
[0021] The present invention has the following advantages:
[0022] The present invention synthesizes a series of MIP-207 catalysts with functional group modification by reflux method. There are abundant and independent Ti-Ox clusters in the MIP-207 structure, which provide a large number of catalytic active sites. The modification of different functional groups also further improves the catalytic efficiency of the catalyst. Therefore, the MIP-207 catalyst with functional group modification described in the present invention has high-efficiency catalytic oxidation desulfurization activity for fuel oil.
[0023] The prepared functional group-modified MIP-207 catalyst has high catalytic performance. When used in catalytic oxidation desulfurization of fuel oil, deep oxidative desulfurization of fuel oil (sulfur content less than 3ppm) can be completed at room temperature (25°C). BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a structural perspective view of MIP-207.
[0025] Figure 2 X-ray diffraction pattern of the functional group-modified MIP-207 catalyst.
[0026] Figure 3 This is the oxidative desulfurization activity diagram of the functional group modified MIP-207 catalyst.
[0027] Figure 4 This is the recycling performance diagram of the functional group-modified MIP-207 catalyst. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto.
[0029] The fuel types used in the following examples are:
[0030] (1) The model oil is prepared by dissolving dibenzothiophene (or 4-methyldibenzothiophene, 4,6-dimethyldibenzothiophene) in dodecane to prepare a model oil having a sulfur content of 200 ppm.
[0031] (2) In a jacketed reaction bottle with magnetic stirring, a catalyst is added to the oil product, and an oxidant and an extractant are added to carry out an oxidative desulfurization reaction under magnetic stirring. During the reaction, the extractant phase and the oil phase are mixed. After the reaction, the extractant phase and the oil phase are allowed to stand for stratification and then separated.
[0032] Gas chromatography (GC-FID) is used to detect the content of sulfides in the oil and calculate the desulfurization rate:
[0033]
[0034] Comparative Example 1:
[0035] The preparation method of MIP-207 is:
[0036] First, 25 mL of acetic acid (HAc) and 25 mL of acetic anhydride (Ac2O) were added to a 100 mL round-bottom flask, and the solution was stirred thoroughly with a magnetic stirrer. 10 mmol (2.10 g) of BTC and 6.75 mmol (2 mL) of isopropyl titanate (Ti(OiPr)4) were added to the solution and stirred for 30 min. The solution was then refluxed at 120 ° C for 12 h. After the reaction was completed, the reactor was cooled to room temperature and the solid was separated from the mixed solution using a centrifuge. The obtained solid was activated in boiling acetone 3 times, each time for 6 h. Finally, the solid was dried in a vacuum oven at 50 ° C for 6 h.
[0037] The content of sulfur compounds (dibenzothiophene) in the oil product is 200ppm. 50mgMIP-207 catalyst, 5mL oil product, 1mL methanol (MeOH) extractant, and 9.6μL H2O2 are added to a double-necked jacket reaction bottle. Stir with a magnetic stirrer and react at room temperature (25℃) for 90min. After the extractant phase and the oil phase are separated after standing and stratification, the desulfurization rate reaches 70.2%.
[0038] Example 1
[0039] The preparation method of MIP-207 with 25% functional group modification is as follows:
[0040] First, prepare 4 sets of 100 mL round-bottom flasks, add 25 mL of acetic acid (HAc) and 25 mL of acetic anhydride (Ac2O) into each round-bottom flask, and use a magnetic stirrer to fully stir the solution, then add 6.75 mmol (2 mL) of titanium source Ti(OiPr)4;
[0041] 7.5mmol (1.57g) BTC was added to the above solutions, and 2.5mmol of different functionalized ligands were added at a 25% molar ratio, namely: 0.42g isophthalic acid (IPA), 0.45g 5-aminoisophthalic acid (5-NH2-IPA), 0.46g 5-hydroxyisophthalic acid (5-OH-IPA), 0.53g 5-nitroisophthalic acid (5-NO2-IPA). After stirring for 30min, the solution was refluxed at 120°C for 12h. After the reaction was completed, the reactor was cooled to room temperature and the solid was separated from the mixed solution using a centrifuge. The obtained solid was activated in boiling acetone 3 times, each time for 6h. Finally, the solid was dried in a vacuum drying oven at 50°C for 6h. The obtained products were recorded as MIP-207-(IPA) 25% 、MIP-207-(5-NH2-IPA) 25% 、MIP-207-(5-OH-IPA) 25% 、MIP-207-(5-NO2-IPA) 25% .
[0042] Example 2
[0043] According to the same synthesis method as Example 1, MIP-207 with 50% functional group modification can be synthesized.
[0044] First, prepare 4 sets of 100 mL round-bottom flasks, add 25 mL of acetic acid HAc and 25 mL of acetic anhydride Ac2O into each round-bottom flask, and use a magnetic stirrer to fully stir the solution, then add 6.75 mmol (2 mL) of titanium source Ti(OiPr)4;
[0045] 5.0mmol (1.05g) BTC was added to the above solutions, and 5.0mmol of different functionalized ligands were added according to the molar ratio of 50%, which were: 0.83g isophthalic acid (IPA), 0.91g 5-aminoisophthalic acid (5-NH2-IPA), 0.91g 5-hydroxyisophthalic acid (5-OH-IPA), 1.01g 5-nitroisophthalic acid (5-NO2-IPA). After stirring for 30min, the solution was refluxed at 120°C for 12h. After the reaction was completed, the reactor was cooled to room temperature and the solid was separated from the mixed solution using a centrifuge. The obtained solid was activated in boiling acetone 3 times, each time for 6h. Finally, the solid was dried in a vacuum drying oven at 50°C for 6h. The obtained products were respectively recorded as MIP-207-(IPA) 50% 、MIP-207-(5-NH2-IPA) 50% 、MIP-207-(5-OH-IPA) 50%、MIP-207-(5-NO2-IPA) 50% .
[0046]
[0047] The application of the functional group-modified MIP-207 catalyst obtained in the present invention in the field of catalytic oxidation fuel desulfurization is as follows:
[0048] Application example 4:
[0049] The content of sulfur compounds (dibenzothiophene) in the oil is 200ppm. 50mgMIP-207-(5-OH-IPA) is added to the double-necked jacketed reaction bottle. 50% Catalyst, 5mL oil, 1mL MeOH extractant, 9.6μL H2O2, stirred with a magnetic stirrer, reacted at room temperature (25℃) for 90min, and the extractant phase and the oil phase were separated after standing and stratification, and the desulfurization rate reached 81.6%.
[0050] Application Example 5:
[0051] The content of sulfur compounds (dibenzothiophene) in the oil is 200ppm. Add 50mgMIP-207-(5-NO2-IPA) into the double-necked jacketed reaction bottle. 50% Catalyst, 5mL oil, 1mL MeOH extractant, 9.6μL H2O2, stirred with a magnetic stirrer, reacted at room temperature (25℃) for 90min, and the extractant phase and the oil phase were separated after standing and stratification, and the desulfurization rate reached 86.5%.
[0052] Application Example 6:
[0053] The content of sulfur compounds (dibenzothiophene) in the oil is 200ppm. Add 50mg MIP-207 (IPA) to the double-necked jacketed reaction bottle. 50% Catalyst, 5mL oil, 1mL MeOH extractant, 9.6μL H2O2, stirred with a magnetic stirrer, reacted at room temperature (25℃) for 90min, and the extractant phase and the oil phase were separated after standing and stratification, and the desulfurization rate reached 88.2%.
[0054] Application Example 7:
[0055] The sulfide (dibenzothiophene) content in the oil is 200ppm. Add 50mg MIP-207-(5-NH2-IPA) into the double-necked jacketed reaction bottle. 50% Catalyst, 5mL oil, 1mL MeOH, 9.6μL H2O2, stirred with a magnetic stirrer, reacted at room temperature (25℃) for 90min, and the extractant phase and the oil phase were separated after standing and stratification. The desulfurization rate reached 98.4%
[0056] Figure 1 This is a structural perspective diagram of MIP-207. Figure 1 The structure of MIP-207 can be clearly seen in the figure: 1,3,5-benzenetricarboxylic acid is used as an organic ligand to connect Ti-O x Octahedral clusters form a typical metal-organic framework structure with a large number of cavities in the structure.
[0057] Figure 2 is the X-ray diffraction (XRD) pattern of functional group-modified MIP-207. Figure 2 It can be seen that the diffraction pattern of the functional group-modified MIP-207 crystal is consistent with the original MIP-207 diffraction pattern, that is, the crystal structure of the functional group-modified MIP-207 has not changed significantly. In the spectrum, the diffraction peaks at 2θ=5.16°, 10.32°, 11.54°, 14.62°, and 15.51° are attributed to the (110), (220), (130), (040), and (330) crystal planes, respectively.
[0058] Figure 3 Oxidative desulfurization activity diagram of functional group modified MIP-207 catalyst. Figure 3 The results show that the catalytic oxidation desulfurization performance of MIP-207 catalysts modified with different functional groups is improved. Among them, MIP-207-(5-NH2-IPA) modified with amino functional groups 50% It has the best catalytic oxidative desulfurization activity, which is attributed to the basic amino group in the catalyst. Specifically, the hydrogen atoms in the basic amino group can produce hydrogen bonds and acid-base interactions with the sulfur atoms of DBT. This makes MIP-207-(5-NH2-IPA) 50% It has excellent catalytic oxidation desulfurization activity and can achieve ultra-deep oxidation desulfurization (98.4%) within 90 minutes at room temperature (25°C).
[0059] Figure 4 This is the recycling performance diagram of the functional group-modified MIP-207 catalyst. Figure 4 It can be seen that MIP-207-(5-NH2-IPA) 50% Under the condition of ensuring deep desulfurization of oil products, the catalyst can be recycled at least five times, has satisfactory recycling performance, and has certain industrial application value.
[0060] The embodiments are preferred implementations of the present invention, but the present invention is not limited to the above-mentioned implementations. Any obvious improvements, substitutions or modifications that can be made by those skilled in the art without departing from the essential content of the present invention belong to the protection scope of the present invention.
Claims
1. A method for preparing a functional group-modified titanium-based metal organic framework material MIP-207, characterized in that: The steps include: Add acetic acid and acetic anhydride to a round-bottom flask and stir thoroughly. Then, add isopropyl titanate as a titanium source to the mixed solution, and then add a functional group-modified ligand and an initial ligand 1,3,5-benzenetricarboxylic acid BTC. After being stirred thoroughly, the mixed solution is refluxed for reaction. After the reaction is completed, the solid powder in the mixed solution is centrifuged and finally the solid is washed, activated and vacuum dried. The functional group-modified ligand is 5-aminoisophthalic acid, 5-nitrobenzeneisophthalic acid, 5-hydroxyisophthalic acid or isophthalic acid; the structural formula is:
2. The preparation method according to claim 1, characterized in that The dosage of isopropyl titanate, functional group modified ligand, initial ligand 1,3,5-benzenetricarboxylic acid BTC, acetic acid and acetic anhydride is 6.75mmol:xmmol:(10-x)mmol:25mL:25mL; wherein x is 2.5-5; namely, the functional group modified ligand accounts for 25%-50% of the total ligand molar amount.
3. The preparation method according to claim 1, characterized in that: The reflux reaction temperature is 120°C and the time is 10 to 14 hours.
4. The preparation method according to claim 1, characterized in that: The washing activation operation is: washing three times with boiling acetone.
5. The preparation method according to claim 1, characterized in that: The vacuum drying temperature is 40-55°C.
6. Use of the functional group modified titanium-based metal organic framework material MIP-207 prepared by the preparation method according to any one of claims 1 to 5 in catalytic oxidation desulfurization of fuel oil.
7. The use according to claim 6, characterized in that The steps are: Add model oil and extractant into a double-necked jacket reaction bottle, add functional group-modified titanium-based metal-organic framework material MIP-207 as a catalyst, place it on a magnetic stirrer, install a condenser above the reaction bottle, and put the reaction bottle into a water bath; use a microinjection needle to add oxidant H2O2 to the reaction bottle to start the reaction, and take out the upper oil phase at equal intervals during the reaction to detect the sulfur content in the oil.
8. The use according to claim 7, characterized in that The dosage ratio of the model oil, the extractant and the catalyst is 5 mL: 1-5 mL: 25-75 mg; the temperature of the water bath is 20-50° C.; and the oxygen-sulfur ratio of the reaction is 2-5.
9. The use according to claim 8, characterized in that The dosage ratio of model oil, extractant and catalyst is 5mL:1mL:50mg; the temperature of the water bath is 25℃; the oxygen-sulfur ratio of the reaction is 3.
Citation Information
Patent Citations
Preparation method and application of organic sulfur conversion catalyst
CN105903491A
Novel preparation method of Fe-MOF (ferrous-metal oxide framework) catalyst and application thereof in desulfurizing field
CN106622381A
Preparation method of NH2-MIL-125 (Ti) desulfurization catalyst with hierarchical hollow structure
CN111921561A
Preparation of cobalt-based metal organic framework immobilized organic catalyst and application of cobalt-based metal organic framework immobilized organic catalyst in field of fuel oil desulfurization
CN113976181A
Method for preparing high-defect titanium-based bimetal organic framework desulfurization catalyst from plasma and application of high-defect titanium-based bimetal organic framework desulfurization catalyst
CN118045634A