Preparation method and application of anti-ultraviolet material MOF-818 for silk fabrics
The single-atom catalyst MOF-818 prepared by spraying on silk fibers solves the aging problem of silk fibers caused by ultraviolet radiation. It significantly delays the aging process by decomposing free radicals and protects the mechanical properties and color of silk fabrics.
Patent Information
- Application Number
- CN202410784234.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-18
AI Technical Summary
Silk fibers are susceptible to degradation, yellowing, brittleness and powdering caused by ultraviolet light irradiation. It is difficult to effectively prevent this aging process with existing technology.
The single atom catalyst MOF-818 was used as a nanomaterial, and MOF-818 was prepared by dissolving ZrOCl2·8H2O, Cu(NO3)2·3H2O and H2PyC in DMF through ultrasonic dissolution, heating, cooling and centrifugation. Prepare a solution in deionized water and spray it on the surface of silk fabrics to absorb ultraviolet light and decompose free radicals.
MOF-818 effectively decomposes dissolved oxygen and reactive oxygen free radicals, inhibits the free radical chain growth reaction caused by ultraviolet radiation of silk fabrics, significantly delays the aging process of silk fibers, and protects the mechanical properties and color of silk fabrics.
Smart Images

Figure CN118725323A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silk fabric protection materials, and in particular to the preparation and application of silk fabric ultraviolet protection material MOF-818. Background Art
[0002] Silk fiber is a natural polymer fiber, but the protein properties of the fiber determine that it is easily degraded by ultraviolet light, turning yellow, brittle, rotten or even powdered. The presence of oxygen is often the main cause of polymer aging. The main effect of polymer exposure to air is oxidative degradation. Under the irradiation of ultraviolet light, the free radicals produced can intensify the effects of light, heat and other factors on polymers, causing more complex degradation and cross-linking reactions. In recent years, the ozone layer in the atmosphere has been severely damaged, and the ultraviolet rays reaching the ground have greatly increased. Silk fabrics are polymer materials composed of proteins, which are easily affected by ultraviolet light factors and degraded and aged. Therefore, people pay attention to the study of the anti-ultraviolet performance of silk fabrics.
[0003] Silk fiber has poor light resistance. Sunlight not only breaks the hydrogen bonds in silk fibroin, but also promotes the photooxidation reaction of silk fibroin. When silk fibroin absorbs the energy of the irradiated light source, the chemical bonds in the molecules break after reaching the dissociation energy, thus destroying the structure of silk. Especially when there are tertiary carbons on the peptide chain, photochemical reactions are very likely to occur under ultraviolet light to generate free radicals. These free radicals will cause the peptide chain to degrade discretely, causing the peptide chain of silk fiber to break, resulting in a decrease in the mechanical properties of silk fabrics and a change in color. This phenomenon will continue to damage silk fibroin even after the light stops.
[0004] For decades, people have been committed to studying the aging mechanism of silk and looking for ways to overcome it through research. Silk cultural relics have been buried underground for a long time and are rarely exposed to sunlight. After being unearthed, they are suddenly exposed to ultraviolet rays from the sun and their damage is aggravated. Therefore, the research on UV-proof materials has become very important. As a new type of nanomaterial, the single-atom catalyst MOF-818 has a low coordination number, a special coordination environment, extremely high atomic utilization, and highly uniform catalytic sites. It is a bridge between homogeneous and traditional heterogeneous catalysts. Studies have found that single-atom catalysts exhibit excellent catalytic activity and can effectively decompose dissolved oxygen or active oxygen free radicals. This feature can be used in the research on antioxidant protection of silk cultural relics. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation method and application of a silk fabric anti-ultraviolet material MOF-818 which has simple operation method, low processing and manufacturing cost, strong operability and good protective effect on silk fabrics.
[0006] The preparation method of the silk fabric anti-ultraviolet material MOF-818 of the present invention comprises the following steps: 1) 84.0-86.0 mg ZrOCl2∙8H2O, 246.0-248.0 mg Cu(NO3)2∙3H2O and 64.0-66.0 mg H2PyC were dissolved in 9-11 mL DMF in sequence, and a uniform mixed solution was obtained under the action of ultrasound. Then, 118-121 μL TFA was added to the mixed solution, heated at 100°C for 10 h, cooled to room temperature, and centrifuged at 10000 rpm for 10 min to collect the obtained product. 2) The product obtained in step 1) was soaked in DMF for 3 days, during which the solvent was exchanged 5 times a day with fresh DMF, and then soaked in acetone for 4 days, 5 times a day. Finally, the sample was vacuum dried at room temperature to obtain MOF-818.
[0007] The application of silk fabric anti-ultraviolet material MOF-818 can be used to protect silk fabrics.
[0008] Application of silk fabric anti-ultraviolet material MOF-818, the application method comprises the following steps: 1) Prepare a 5 mg / ml solution of the synthesized MOF-818 material in deionized water. Add MOF-818 powder into deionized water and mix well. 2) Put the solution prepared in step 1) into a spray bottle, spray the MOF-818 material aqueous solution on the surface of the silk fabric with the spray bottle, and spread it flat to dry; 3) The silk fabric sprayed with MOF-818 material was placed in a UV aging box irradiated with a 340nm ultraviolet wavelength for 20 days; at the same time, the silk fabric sample block that had not been treated was also placed in a UV aging box irradiated with a 340nm ultraviolet wavelength.
[0009] In the step 3), the temperature and humidity of the UV aging box are set to 25°C and 65% respectively.
[0010] Beneficial effects of the present invention: As a new type of nanomaterial, MOF-818 has a low coordination number, a special coordination environment, extremely high atomic utilization, and highly uniform catalytic sites. It is a bridge between homogeneous and traditional heterogeneous catalysts. Based on the excellent catalytic activity of single-atom catalysts, it can effectively decompose dissolved oxygen or active oxygen free radicals, eliminate free radicals generated by silk fabrics after ultraviolet radiation, inhibit free radical chain growth reactions, and effectively protect silk fabrics. It is of great significance to the ultraviolet protection of silk fabrics in my country. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 This is the transmission electron microscope (TEM) image of MOF-818 of the present invention; Figure 2 This is the X-ray diffraction pattern of MOF-818 of the present invention; Figure 3 This is the HAADF-STEM image of MOF-818 of the present invention; Figure 4 This is a diagram of the SOD-like enzyme activity of MOF-818 of the present invention; Figure 5 This is a graph showing the concentration of MOF-818 and the activity of the SOD-like enzyme; Figure 6 is a scanning electron microscope image (SEM) of MOF-818 in the present invention; Figure 7 The XPS photoelectron spectrum of MOF-818 in the present invention; Figure 8 is the EDX spectrum of MOF-818 in the present invention; Fig. 9 It is a high-resolution image of the C 1s XPS spectrum of MOF-818 in the present invention; Fig.10 It is a high-resolution image of the O 1s XPS spectrum of MOF-818 in the present invention; Fig.11 This is a high-resolution image of the N 1s XPS spectrum of MOF-818 in the present invention. Fig.12 is the infrared absorption diagram of MOF-818 in the present invention; Fig.13 It is a high-resolution image of the Cu 2p XPS spectrum of MOF-818 in the present invention; Fig.14 It is a high-resolution image of the Zr 3d XPS spectrum of MOF-818 in the present invention; Fig.15 is the Brunauer-Emmet-Teller (BET) surface area of MOF-818 in the present invention; Fig.16 This is the pore size distribution diagram of MOF-818 in the present invention; Fig.17 This is a color difference diagram of the silk fabric of the present invention before and after being protected by MOF-818; Fig.18 This is a surface electron microscope image (SEM) of the unaged silk fabric of the present invention; Fig.19 This is a surface electron microscope image (SEM) of the silk fabric of the present invention after aging; Fig. 20This is a surface electron microscope image (SEM) of the silk fabric of the present invention after being protected by MOF-818; Fig.21 IR spectra of different samples in the present invention; Fig. 22 It is the X-ray diffraction pattern of the same sample in the present invention. DETAILED DESCRIPTION
[0012] The present invention will be further described below in conjunction with the accompanying drawings.
[0013] The method for preparing the silk fabric ultraviolet protection material MOF-818 of the present invention comprises the following steps: 1) 85.0 mg ZrOCl2∙8H2O, 248.0 mg Cu(NO3)2∙3H2O and 65.0 mg H2PyC were dissolved in 10 mL DMF in sequence, and a uniform mixed solution was obtained under the action of ultrasound. Then, 120 μL TFA was added to the mixed solution, and the mixture was heated at 100 °C for 10 h. After cooling to room temperature, the mixture was centrifuged at 10000 rpm for 10 min to collect the obtained product. 2) The product obtained in step 1) was soaked in DMF for 3 days, during which the solvent was exchanged 5 times a day with fresh DMF, and then soaked in acetone for 4 days, 5 times a day. Finally, the sample was vacuum dried at room temperature to obtain MOF-818.
[0014] Among them: TEM image of MOF-818, Figure 1 and the corresponding element map image Figure 3 It shows that Zr, N, O, and Cu are evenly distributed in the selected area, showing an octahedral structure; the X-ray diffraction pattern, i.e. Figure 2 As shown in Figure 2, the peaks at 3.01, 4.91, 5.99 and 6.89 correspond to the crystal structures of 111, 220, 222 and 400 faces, respectively. This indicates that MOF-818 was successfully prepared. We further used a SOD detection kit to study the SOD-like activity of MOF-818, and used a UV-visible spectrophotometer to detect it at about 450nm. When MOF-818-like was added to the system, it reacted with O2 •- A disproportionation reaction occurs to generate hydrogen peroxide (H2O2) and oxygen (O2). Figure 2 As shown in Figure 2, MOF-818 exhibited excellent SOD-like enzyme activity, and as the concentration of MOF-818 increased from 0.1 ug / mL to 10 ug / mL, the activity also increased. Figure 5 shown.
[0015] The application of silk fabric anti-ultraviolet material MOF-818 can be used to protect silk fabrics.
[0016] Application of silk fabric anti-ultraviolet material MOF-818, the application method comprises the following steps: 1) Prepare a 5 mg / ml solution of the synthesized MOF-818 material in deionized water. Add MOF-818 powder into deionized water and mix well. 2) Put the solution prepared in step 1) into a spray bottle, spray the MOF-818 material aqueous solution on the surface of the silk fabric with the spray bottle, and spread it flat to dry; 3) The silk fabric sprayed with MOF-818 material was placed in a UV aging box irradiated with a 340nm ultraviolet wavelength for 20 days; at the same time, the silk fabric sample block that had not been treated was also placed in a UV aging box irradiated with a 340nm ultraviolet wavelength.
[0017] In the step 4), the temperature and humidity of the UV aging box are set to 25°C and 65% respectively.
[0018] The following uses color difference, infrared, diffraction and other methods to evaluate the protective effect of the single-atom catalyst MOF-818 in terms of color change and degradation degree of silk fabrics after ultraviolet irradiation; 1) Color difference test The silk fabric was tested for color difference before application (select three areas), tested for color difference (in the same area), and then ∆E was calculated. Fig.17 As shown, the calculation formula is as follows: , ∆L, ∆a, ∆b are the differences of L, a, and b before and after the measurement, respectively. The color difference change value of silk with MOF-818 added is smaller than that of untreated silk, indicating that the protective agent plays a key role in UV protection. Silk is a natural polymer fiber, but the protein nature of the fiber determines that it is susceptible to ultraviolet light and photochemical reactions. In particular, when there are tertiary carbons on the peptide chain, free amino acids are easily produced in the photochemical reaction, and yellow substances are also produced. These substances will change the color of silk fibers and ultimately lead to changes in the color of silk; MOF-818 can catalyze the O2 produced during the reaction. •- It can remove free radicals and reduce the damage of ultraviolet rays to silk.
[0019] 2) Morphology analysis Depend on Fig.18 It can be seen that the surface of the silk fabric sample that has not been aged is smooth. Except for a few places, the overall thickness is relatively uniform, and there is no obvious fracture or crack. The sample that has been light aged for 200 hours, Fig.19 As shown in the figure, cracks in the same direction as the fiber axis have appeared on the sample surface, and some fibers have split, indicating that some silk fabrics have aged. The sample of silk fabrics treated with MOF-818 and photo-aged for 200 hours, Fig. 20As shown, there are no obvious cracks and fractures on the surface of the sample, which indicates that MOF-818 has a certain protective effect on silk fibers under ultraviolet radiation.
[0020] 3) Infrared analysis Table 1 Infrared characteristic absorption bands of test samples The blank sample, the aged sample after MOF-818 treatment, and the pure aged sample were tested by infrared spectroscopy. The results showed that the samples all showed the characteristic absorption band of protein fiber. Fig.21 As shown, at 3270cm -1 -NH stretching vibration, 1620cm -1 、1512cm -1 、1230cm -1 Nearby amide I, II, and III bands, 1060 cm -1 The amide IV band at 1620 cm -1 The amide I band belongs to the β-sheet, 1230 cm -1 The amide III bands belong to random coil and α-helix. -1 、1440cm -1 、1160cm -1 A strong absorption peak also appears at , which overall shows that the tested sample conforms to the infrared spectrum characteristics of silk fiber, and the tested sample is determined to be silk fiber.
[0021] As shown in Table 1, the aged samples treated with MOF-818 and the pure aged samples have a -1 The absorption peaks near the blank sample are slightly higher than the absorption peak of the blank sample, but the absorption peak of the amide II band is slightly weakened after aging treatment. After aging treatment, the silk protein molecules of the tested samples are damaged to a certain extent, and some hydrogen bonds are destroyed, resulting in a decrease in the -NH peak that forms hydrogen bonds; in general, the displacement results of the aged samples treated with MOF-818 are smaller than those of the pure old samples, which shows that MOF-818 plays a certain protective role in the aging of silk fabrics and protects the molecular structure of silk protein fibers.
[0022] 4) Diffraction analysis Table 2 Correlation values of X-ray diffraction patterns of different samples The blank sample, the aged sample after MOF-818 treatment, and the pure aged sample were analyzed by X-ray diffraction. Fig. 22As shown in Figure 2 and Table 2, a comparative test was conducted and it was found that after aging treatment, the pure aged sample had the highest crystallinity. The crystallinity of the aged sample treated with MOF-818 increased, but was lower than that of the pure aged sample. When the silk fiber aged and degraded, the non-crystalline area degraded first, resulting in an increase in the crystallinity of the silk fiber. However, with the extension of aging time and the deepening of degradation, the crystalline area began to degrade, the spatial arrangement weakened, and the crystallinity decreased. The results show that when silk is exposed to ultraviolet radiation, the applied MOF-818 can slow down the aging rate of silk to a certain extent.
[0023] 5) Amino acid analysis Silk products are mainly composed of glycine and alanine, followed by serine and tyrosine, and aspartic acid, glutamine, threonine, isoleucine and other amino acids. By comparing the contents of various amino acids in blank samples, aged samples treated with MOF-818, and pure aged samples before and after aging, it was found that the content of glycine in the β-folding area and alanine in the crystalline area of silk fibers decreased after aging. Serine is mainly present in sericin, while tyrosine and phenylalanine are mostly in the non-crystalline area, and their content decreases most significantly during the aging process.
[0024] As an aromatic substance, tyrosine is easily oxidized by heat. The side gene space steric hindrance in its own structure, mainly in the non-crystalline area, is more likely to be lost, resulting in a significant decrease in the tyrosine content before and after aging. From the ratio of glycine to tyrosine content, it can be seen that the Gly / Tyr ratio increased from 3.603 to 3.744 before and after aging, while the ratio after MOF-818 treatment was 3.741. The increase in this ratio indicates that the content of large side amino acids in the aged sample has decreased, and MOF-818 treatment can effectively delay the aging process of silk fibers.
[0025] Table 3 Amino acid content of different samples during aging
Claims
1. Preparation method of silk fabric anti-ultraviolet material MOF-818, Features: The method comprises the following steps: 1) 84.0-86.0 mgZrOCl 2 ∙8H 2 O, 246.0 -248.0 mg Cu(NO 3 ) 2 ∙3H 2 O and 64.0 -66.0mgH 2 PyC was dissolved in 9-11 mL DMF in turn, and a uniform mixed solution was obtained under the action of ultrasound. Then, 118-121 μL of TFA was added to the mixed solution, heated at 100 °C for 10 h, cooled to room temperature, and centrifuged at 10000 rpm for 10 min to collect the obtained product; 2) The product obtained in step 1) was soaked in DMF for 3 days, during which the solvent was exchanged 5 times a day with fresh DMF, and then soaked in acetone for 4 days, 5 times a day. Finally, the sample was vacuum dried at room temperature to obtain MOF-818.
2. The application of the silk fabric anti-ultraviolet material MOF-818 as claimed in claim 1, Features: Used to protect silk fabrics.
3. The use of the silk fabric anti-ultraviolet material MOF-818 as claimed in claim 2, It is characterized in that The application method comprises the following steps: 1) Mix the synthesized MOF-818 material in deionized water to prepare a 5 mg / ml solution. Add MOF-818 powder into deionized water and mix well. 2) Put the solution prepared in step 1) into a spray bottle, spray the MOF-818 material aqueous solution on the surface of the silk fabric with the spray bottle, and spread it flat to dry; 3) The silk fabric sprayed with MOF-818 material was placed in a UV aging box irradiated with a 340nm ultraviolet wavelength for 20 days; at the same time, the silk fabric sample block that had not been treated was also placed in a UV aging box irradiated with a 340nm ultraviolet wavelength.
4. The use of the silk fabric anti-ultraviolet material MOF-818 as claimed in claim 3, Features: In the step 3), the temperature and humidity of the UV aging box are set to 25°C and 65% respectively.
Citation Information
Patent Citations
Anti-tumor pharmaceutical composition and application thereof
CN113893263A
Anti-ultraviolet super-hydrophobic fabric and preparation method thereof
CN114990885A
Synthesis method of MOF-on-MOF material and application of chlorpyrifos detection
CN116284810A
Modified sericin anti-ultraviolet coating and preparation method thereof
CN116377728A
Electrospun nanofibrous polymer membrane for use in air filtration applications
US20230167591A1
Cited By
Method for simply, conveniently, mildly and efficiently preparing MOF-818
CN121203171A