Hyperbranched lignin-based piperazine phosphorus-containing flame-retardant polyolefin and preparation method thereof

Through the preparation of hyperbranched lignin-based piperazine phosphorus-containing flame retardants and polyolefin melt compounding, the problem of balancing the flammability and performance of polypropylene materials has been solved, and low-cost and efficient flame retardant effects and mechanical properties have been improved. Suitable for a variety of polyolefin materials.

CN118725338APending Publication Date: 2024-10-01CHANGCHUN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410765787.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The flammability of polypropylene materials and the difficulty of balancing flame retardant properties, droplet properties and mechanical properties, especially when meeting the application requirements of polyolefin materials, traditional flame retardants have problems of high cost and environmental impact.

Method used

Hyperbranched lignin-based piperazine phosphorus-containing flame retardant is grafted with lignin through Mannich reaction, and the synergistic effect of phosphorylation and nitrogen source is used to prepare a halogen-free intumescent flame retardant, which is melted with polyolefin. Compounded to form highly efficient flame retardant polyolefin materials.

Benefits of technology

It achieves low-cost, green, halogen-free flame retardant effect, significantly improves the flame retardant and mechanical properties of polyolefin materials, and is suitable for a variety of polyolefin materials, especially non-polar polyolefins such as polyethylene and polypropylene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725338A_ABST
    Figure CN118725338A_ABST
Patent Text Reader

Abstract

The invention provides hyperbranched lignin-based piperazine phosphorus-containing flame-retardant polyolefin and a preparation method thereof. The preparation method comprises the following steps: reacting lignin, piperazine and phosphoric acid to obtain an intumescent synergistic flame retardant; and carrying out melt extrusion compounding on the flame retardant and polyolefin to prepare flame-retardant polyolefin. The flame retardant contains lignin and phosphorus and nitrogen elements, and has excellent char forming and flame retardant effects; the flame retardant contains a nitrogen element and can provide a nitrogen source in the flame retardant; the efficient flame retardant with a synergistic effect is formed. Meanwhile, lignin charring can enhance the barrier effect of the material, and meanwhile, the mechanical property of the material is improved. The flame retardant synthesized from lignin is low in cost and environment-friendly, and the flame-retardant polyolefin composite material is excellent in comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and in particular to a hyperbranched lignin-based piperazine phosphorus-containing flame-retardant polyolefin and a preparation method thereof. Background Art

[0002] Polyolefin materials are colorless, translucent, thermoplastic, lightweight general-purpose plastics, mainly including polypropylene (PP), low-density polyethylene (LDPE), etc. With chemical resistance, heat resistance, electrical insulation, high-strength mechanical properties and good high-wear processing properties, polyolefins are rapidly being widely used in many fields such as machinery, automobiles, electronic appliances, construction, agriculture, forestry, fishery and food industries. In addition, because of its certain plasticity, polyolefin materials are gradually replacing wooden products, and high-strength toughness and high wear resistance have gradually replaced the mechanical functions of metals. On the other hand, polyolefins have good grafting and composite functions, and have huge application space in concrete, textiles, packaging, agriculture, forestry and fishery.

[0003] In modern production and life, polyolefin materials are widely used in automobile interior and exterior trims, home decoration, etc. However, with the huge market for polypropylene, the flammability of polypropylene is also a major problem that needs to be solved urgently. The flame retardancy of polypropylene is mainly achieved by introducing flame retardant components, that is, additive flame retardant technology. The added flame retardant components are called additive flame retardants. It can be evenly dispersed in the polyolefin matrix to prevent the occurrence of combustion, or it can be added to the raw materials. Flame retardant elements such as nitrogen, phosphorus or halogens participate in combustion partially or completely, and the generated substances play a gas phase and condensed phase flame retardant role. Commonly used flame retardants for polyolefins can be divided into halogen flame retardants, phosphorus flame retardants, nitrogen flame retardants, inorganic flame retardants and intumescent flame retardants according to the flame retardant components.

[0004] Lignin contains a variety of functional groups, such as alcoholic hydroxyl, phenolic hydroxyl, carbonyl, carboxyl and a large number of aromatic structures. Lignin accounts for a considerable proportion of plant components and is a natural renewable polymer material. The wastewater produced by the pulping process contains a large amount of lignin. Through the comprehensive utilization of this part of lignin, the damage to the ecological environment can be eliminated and low-cost and efficient utilization can be achieved.

[0005] Based on the above, developing a lignin-based green flame retardant that can efficiently enhance thermal insulation, smoke suppression and flame retardancy while meeting the flame retardancy, droplet performance and mechanical properties of polyolefin materials has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] In order to solve the above technical problems, a hyperbranched lignin-based piperazine phosphorus-containing flame-retardant polypropylene and a preparation method thereof include the following steps:

[0007] (1) Dissolve 16.50-17.85 g of piperazine in 65-75 mL of deionized water to obtain a piperazine aqueous solution.

[0008] (2) Add 25-32 mL of formaldehyde solution to the piperazine aqueous solution in step (1) and react at 50-60° C. for 0.5-0.8 h.

[0009] (3) Dissolve 5 g of lignin in water with a pH of 8.5 to 9.5, add the dissolved lignin to the solution after the reaction in step (2), and react at 55 to 65° C. for 4 to 5 hours.

[0010] (4) After the reaction is completed, the product obtained in step (3) is allowed to stand and cool to 4-10°C.

[0011] (5) Add 25-30 mL of 2M hydrochloric acid to the reaction solution obtained after standing in step (4) to adjust the pH value of the system to 3-4, thereby obtaining a yellow-brown solution.

[0012] (6) adding deionized water to adjust the pH value of the system to a range of 6 to 7, filtering, drying in a vacuum oven at 70 to 75° C., and pulverizing to obtain nitrogen-containing lignin-based intermediate product LPI powder.

[0013] (7) Take 5-10 g of nitrogen-containing lignin-based intermediate LPI powder, dissolve it in 100-120 mL of water containing 5-8 mL of acetic acid, and stir it at 25-30° C. for 0.5-1 h.

[0014] (8) Add 85-100 mL of 85% phosphoric acid solution to the LPI solution obtained in step (7), and continue the reaction at 50-60° C. for 3-5 h.

[0015] (9) Add the pre-product obtained in step (8) into ethanol to precipitate the product to obtain brown floccules, wash the product with ethanol for multiple times, and dry the product at 60-75° C. for 15-24 hours. After crushing, a hyperbranched lignin-based piperazine phosphorus-containing flame retardant (LPIP) is obtained.

[0016] Furthermore, the lignin is any one of enzymatic lignin, organic solvent lignin, alkali lignin and sodium lignin sulfonate.

[0017] The present invention further provides a flame retardant polyolefin, wherein the flame retardant polyolefin contains the aforementioned hyperbranched lignin-based piperazine phosphorus-containing flame retardant (LPIP).

[0018] The present invention also provides a method for preparing a flame-retardant polyolefin, wherein the flame-retardant polyolefin is prepared by melt-compounding a polyolefin with the aforementioned hyperbranched lignin-based piperazine phosphorus-containing flame retardant (LPIP). The preparation method specifically comprises: adding a hyperbranched lignin-based piperazine phosphorus-containing flame retardant (LPIP), a polyolefin and a coupling agent into a twin-screw extruder, mixing, melt-extruding, granulating, and injection molding to obtain a flame-retardant polyolefin material.

[0019] Finally, the present invention also provides application of the hyperbranched lignin-based piperazine phosphorus-containing flame retardant (LPIP) in flame-retardant polyolefin.

[0020] Furthermore, the coupling agent is any one of γ-aminopropyltriethoxysilane (KH-550), γ-glycidyloxypropyltrimethoxysilane (KH-560), γ-methacryloxypropyltrimethoxysilane (KH-570), and maleic anhydride grafted polypropylene (MAPP).

[0021] Furthermore, the weight ratio of the polyolefin, the lignin-based melamine phosphorus-containing flame retardant, and the silane coupling agent is 74-80:16-22:4.

[0022] Beneficial Effects of the Invention

[0023] The present invention provides a hyperbranched lignin-based piperazine phosphorus-containing flame-retardant polyolefin and a preparation method thereof. The hyperbranched lignin-based piperazine phosphorus-containing flame retardant (LPIP) of the present invention is a halogen-free flame retardant, and the phosphorus element used and the nitrogen element in piperazine are both green compared to halogen flame retardants. The present invention utilizes piperazine, and formaldehyde is grafted with lignin by Mannich reaction for phosphorylation, and finally obtains a halogen-free lignin-based flame retardant with synergistic effects of nitrogen and phosphorus. Because lignin is a very good carbon-forming agent, it has a good effect on synergistic flame retardancy, thereby forming an intumescent flame retardant carbon-forming agent, and piperazine and phosphonic acid provide a phosphorus source and a nitrogen source for the system, and under the synergistic effect of the three, the optimal flame retardant effect is obtained. Compared with traditional flame retardants, the addition of lignin greatly reduces the cost of flame retardants. The lignin-based flame retardant prepared by the present invention is applied to polyolefins to obtain a low-cost flame-retardant polyolefin material with excellent performance. In addition, the flame retardant obtained has good flame retardancy for polyethylene, polypropylene and other non-polar polyolefins, and has an enhancing effect on their mechanical properties. Therefore, the flame retardant obtained has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a reaction synthesis route for hyperbranched lignin-based piperazine phosphorus-containing flame retardant (LPIP). DETAILED DESCRIPTION

[0025] The technical solutions in the present invention are described clearly and completely below in conjunction with specific embodiments. Of course, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention.

[0026] Example 1

[0027] Dissolve 16.50-17.85g piperazine in 65-75mL deionized water to obtain a piperazine aqueous solution. Take 25-32mL formaldehyde solution and add it to the piperazine aqueous solution, and react at 50-60℃ for 0.5-0.8h. Dissolve 5g lignin in water with a pH of 8.5-9.5, add it to the reacted solution after dissolution, and react at 55-65℃ for 4-5h. After the reaction is completed, the product obtained by the reaction is allowed to stand and cooled to 4-10℃. Add 25-30mL 2M hydrochloric acid to the reaction solution obtained after standing to adjust the pH value of the system to 3-4, and obtain a yellow-brown solution. Add deionized water to adjust the pH value of the system to 6-7, filter, dry in a vacuum oven at 70-75℃, and crush to obtain nitrogen-containing lignin-based intermediate product LPI powder.

[0028] Example 2

[0029] Take 5-10g of nitrogen-containing lignin-based intermediate product LPI powder, dissolve it in 100-120mL water containing 5-8mL acetic acid, and stir it at 25-30°C for 0.5-1h. Add 85-100mL of 85% phosphoric acid solution to the LPI solution, and continue to react at 50-60°C for 3-5h. Add the pre-product to ethanol to precipitate the product to obtain brown floccules, wash it with ethanol several times, and dry it at 60-75°C for 15-24h. After crushing, a hyperbranched lignin-based piperazine phosphorus flame retardant (LPIP) is obtained.

[0030] Example 3

[0031] Weigh 100g of polypropylene (PP), add it to the hopper, press it evenly, and put it into the injection molding machine at 215-235℃ to obtain the tensile strength, oxygen index and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index and UL-94 of the polypropylene material are shown in Table 1.

[0032] Example 4

[0033] Weigh 100g of polypropylene (PE), add it to the hopper, press it evenly and put it into the injection molding machine at 215-235℃ to obtain the tensile strength, oxygen index and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index and UL-94 of the polypropylene material are shown in Table 1.

[0034] Comparative Example 1

[0035] Weigh 80.0g of polypropylene, 16.0g of lignin-based piperazine phosphorus flame retardant (LPIP), and 4.0g of γ-aminopropyl triethoxysilane (KH-550), mix them evenly, add them to a twin-screw extruder for extrusion granulation, and obtain PP / LPIP-16 sample pellets. Put the PP / LPIP-16 sample pellets into a hopper, press them evenly, and then put them into an injection molding machine at 215-235°C to obtain tensile strength, oxygen index, and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index, and UL-94 of the polypropylene material are tested as shown in Table 1.

[0036] Comparative Example 2

[0037] Weigh 78.0g of polypropylene, 18.0g of lignin-based piperazine phosphorus flame retardant (LPIP), and 4.0g of γ-aminopropyl triethoxysilane (KH-550), mix them evenly, and add them to a twin-screw extruder for extrusion granulation to obtain PP / LPIP-18 sample pellets. Put the PP / LPIP-18 sample pellets into a hopper, press them evenly, and then put them into an injection molding machine at 215-235°C to obtain tensile strength, oxygen index, and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index, and UL-94 of the polypropylene material are tested as shown in Table 1.

[0038] Comparative Example 3

[0039] Weigh 76.0g of polypropylene, 20.0g of lignin-based piperazine phosphorus flame retardant (LPIP), and 4.0g of γ-aminopropyl triethoxysilane (KH-550), mix them evenly, add them to a twin-screw extruder for extrusion granulation, and obtain PP / LPIP-20 sample pellets. Put the PP / LPIP-20 sample pellets into a hopper, press them evenly, and then put them into an injection molding machine at 215-235°C to obtain tensile strength, oxygen index, and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index, and UL-94 of the polypropylene material are tested as shown in Table 1.

[0040] Comparative Example 4

[0041] Weigh 74.0g of polypropylene, 22.0g of lignin-based piperazine phosphorus flame retardant (LPIP), and 4.0g of γ-aminopropyl triethoxysilane (KH-550), mix them evenly, and add them to a twin-screw extruder for extrusion granulation to obtain PP / LPIP-22 sample pellets. Put the PP / LPIP-22 sample pellets into a hopper, press them evenly, and then put them into an injection molding machine at 215-235°C to obtain tensile strength, oxygen index, and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index, and UL-94 of the test materials are shown in Table 1.

[0042] Comparative Example 5

[0043] Weigh 80.0g of low-density polyethylene, 16.0g of lignin-based piperazine phosphorus flame retardant (LPIP), and 4.0g of γ-aminopropyl triethoxysilane (KH-550), mix them evenly, and add them to a twin-screw extruder for extrusion granulation to obtain PE / LPIP-16 sample pellets. Put the PP / LPIP-16 sample pellets into a hopper, press them evenly, and then put them into an injection molding machine at 215-235°C to obtain tensile strength, oxygen index, and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index, and UL-94 of the test materials are shown in Table 1.

[0044] Comparative Example 6

[0045] Weigh 78.0g of low-density polyethylene, 18.0g of lignin-based piperazine phosphorus flame retardant (LPIP), and 4.0g of γ-aminopropyl triethoxysilane (KH-550), mix them evenly, and add them to a twin-screw extruder for extrusion granulation to obtain PE / LPIP-18 sample pellets. Put the PP / LPIP-18 sample pellets into a hopper, press them evenly, and put them into an injection molding machine at 215-235°C to obtain tensile strength, oxygen index, and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index, and UL-94 of the test materials are shown in Table 1.

[0046] Comparative Example 7

[0047] Weigh 76.0g of low-density polyethylene, 20.0g of lignin-based piperazine phosphorus flame retardant (LPIP), and 4.0g of γ-aminopropyl triethoxysilane (KH-550), mix them evenly, and add them to a twin-screw extruder for extrusion granulation to obtain PE / LPIP-20 sample pellets. Put the PP / LPIP-20 sample pellets into a hopper, press them evenly, and then put them into an injection molding machine at 215-235°C to obtain tensile strength, oxygen index, and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index, and UL-94 of the test materials are shown in Table 1.

[0048] Comparative Example 8

[0049] Weigh 74.0g of low-density polyethylene, 22.0g of lignin-based piperazine phosphorus flame retardant (LPIP), and 4.0g of γ-aminopropyl triethoxysilane (KH-550), mix them evenly, and add them to a twin-screw extruder for extrusion granulation to obtain PE / LPIP-22 sample pellets. Put the PP / LPIP-22 sample pellets into a hopper, press them evenly, and then put them into an injection molding machine at 215-235°C to obtain tensile strength, oxygen index, and UL-94 test specimens. The tensile strength, tensile modulus, oxygen index, and UL-94 of the test materials are shown in Table 1.

[0050] Performance Testing

[0051] (1) Tensile performance test: The test was conducted in accordance with the national standard GB / T 1040.1-2006.

[0052] (2) Limiting oxygen index test: The test is carried out in accordance with GB / T 2406.2-2009.

[0053] (3) UL-94 vertical flame test: The standard is tested in accordance with GB / T2408-2008.

[0054] Table 1: Tensile strength, tensile modulus, oxygen index and UL-94 of flame-retardant polypropylene prepared in Comparative Examples 1 to 4 and Example 2.

[0055] Table 1: Comparison of mechanical properties and flame retardant properties of flame retardant polypropylene composite materials prepared in Examples 3 to 4 and Comparative Examples 1 to 8

[0056]

[0057]

[0058] The flame retardant polyolefin composite materials prepared in Examples 3 and 4 of the present invention and Comparative Examples 1 to 8, the tensile strength, tensile modulus, oxygen index and UL-94 are shown in Table 1. It can be seen from the data in Table 1 that the addition of LPIP significantly improves the tensile strength, tensile modulus, oxygen index and UL-94 grade of non-polar resins PP and LDPE, and it is preferred that the addition amount of LPIP is 16 to 22 parts by weight based on 100 parts by weight of the resin composition. Within this range, the tensile strength and tensile modulus of the polypropylene composite material are significantly improved with the increase of the content of the flame retardant; in addition, the oxygen index of the composite material also increases with the increase of the amount of the flame retardant, reaching the level of non-flammability.

[0059] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A hyperbranched lignin-based piperazine phosphorus-containing flame retardant, which is prepared by reacting lignin, piperazine and phosphoric acid.

2. The method for preparing the hyperbranched lignin-based piperazine phosphorus-containing flame retardant according to claim 1, characterized in that it is prepared by the following method: (1) Dissolve 16.50-17.85 g of piperazine in 65-75 mL of deionized water to obtain a piperazine aqueous solution. (2) Add 25-32 mL of formaldehyde solution to the piperazine aqueous solution in step (1) and react at 50-60° C. for 0.5-0.8 h. (3) Dissolve 5 g of lignin in water with a pH of 8.5 to 9.5, add the dissolved lignin to the solution after the reaction in step (2), and react at 55 to 65° C. for 4 to 5 hours. (4) After the reaction is completed, the product obtained in step (3) is allowed to stand and cool to 4-10°C. (5) Add 25-30 mL of 2M hydrochloric acid to the reaction solution obtained after standing in step (4) to adjust the pH value of the system to 3-4, thereby obtaining a yellow-brown solution. (6) adding deionized water to adjust the pH value of the system to a range of 6 to 7, filtering, drying in a vacuum oven at 70 to 75° C., and pulverizing to obtain nitrogen-containing lignin-based intermediate product LPI powder. (7) Take 5-10 g of nitrogen-containing lignin-based intermediate LPI powder, dissolve it in 100-120 mL of water containing 5-8 mL of acetic acid, and stir it at 25-30° C. for 0.5-1 h. (8) Add 85-100 mL of 85% phosphoric acid solution to the LPI solution obtained in step (7), and continue the reaction at 50-60° C. for 3-5 h. (9) Add the pre-product obtained in step (8) into ethanol to precipitate the product to obtain brown floccules, wash the product with ethanol for multiple times, and dry the product at 60-75° C. for 15-24 hours. After crushing, a hyperbranched lignin-based piperazine phosphorus-containing flame retardant (LPIP) is obtained.

3. A hyperbranched lignin-based piperazine phosphorus-containing flame retardant according to claim 1, Features: The lignin is any one of enzymatic lignin, organic solvent lignin, alkali lignin and sodium lignin sulfonate.

4. Use of the hyperbranched lignin-based piperazine phosphorus-containing flame retardant according to claim 1 or 2 or the hyperbranched lignin-based piperazine phosphorus-containing flame retardant prepared by the preparation method according to any one of claim 3 in polyolefins.