Preparation method and application of organic conductive gel
By dissolving metal salts with low-level polycarboxylic acids and low-level polyols in organic solutions, and polymerizing with acrylamide, a polyacrylamide organic conductive gel is formed, which solves the problems of conductivity and stability and achieves high transparency and stretchability. and frost resistance, suitable for fields such as flexible electronic devices.
Patent Information
- Application Number
- CN202310338076.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
Existing organic conductive gels have low solubility of metal salts in polymer solutions, resulting in reduced conductivity. Moreover, hydrogels are prone to water loss and deformation, and have poor performance stability. It is difficult to meet the requirements of stretchability, self-healing, and anti-freeze of flexible electronic devices. properties and conductivity requirements.
By dissolving the metal salt, low-level polycarboxylic acid and low-level polyol in a mixed organic solution, and polymerizing acrylamide to form a polyacrylamide organic conductive gel, ensuring that the metal salt is dissolved in a small molecule organic solvent and generating a conductive gel with good conductivity. polymer.
The prepared organic conductive gel has high transparency, good stretchability, frost resistance, self-healing and conductivity, and is suitable for flexible electronic devices, sensors and wearable devices.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material processing, and in particular relates to a preparation method and application of an organic conductive gel. Background Art
[0002] With the development of intelligent flexible electronic devices, the application research of stretchable and self-healing electrodes and electrolyte materials has attracted more and more attention. The first is the application research of conductive hydrogels, which gradually solved the problems of poor mechanical properties and poor frost resistance. However, hydrogels are prone to water loss and deformation, resulting in poor performance stability. Therefore, organic conductive gels have been studied and developed. Organic conductive gels usually use solvent replacement to convert hydrogels into organic gels, but the solubility of metal salts in organic solvents is low, and the ion concentration in organic gels is low, resulting in decreased conductivity. Directly mixing metal salts into polymer solutions will also precipitate from organic gels under the action of organic solvents, and the conductivity will also drop sharply. Therefore, in response to the development requirements of flexible electronic devices, it is urgent to develop stretchable, self-healing, frost-resistant, stable, and conductive organic conductive gels. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a method for preparing an organic conductive gel, wherein a metal salt is dissolved in a small molecule organic solvent, and then acrylamide is polymerized to form a polymer organic conductive gel containing a metal salt. The prepared organic conductive gel has high transparency, good stretchability, antifreeze, self-healing property, conductivity and stability.
[0004] The present invention provides the following technical solutions: A method for preparing an organic conductive gel comprises the following steps: S1. dissolving a metal salt and a low polycarboxylic acid in a low polyol to obtain a mixed organic solution A, wherein the metal salt is one or more of lithium bromide, lithium chloride, potassium bromide, potassium chloride, sodium chloride, and sodium dihydrogen phosphate; the low polycarboxylic acid is any one of oxalic acid, malic acid, and tartaric acid; and the low polyol is one or more of ethylene glycol, propylene glycol, and glycerol; S2. dissolving acrylamide powder in a lower polyol to obtain an organic solution B, wherein the lower polyol is one or more of ethylene glycol, propylene glycol and glycerol; S3. Mix the organic solution A and the organic solution B, stir them evenly, degas them in vacuum, and let them stand for a short time to allow the acrylamide to polymerize and generate polyacrylamide organic conductive gel.
[0005] Preferably, the amount of the metal salt in S1 is 10 wt% to 20 wt%.
[0006] Preferably, the mass ratio of the lower polycarboxylic acid to the lower polyol in S1 is 1:1-5.
[0007] Preferably, the mass ratio of acrylamide to lower polyol in S2 is 1-1.5:1.
[0008] Preferably, the mass ratio of the organic solution A to the organic solution B in S3 is 1:1-2.
[0009] Furthermore, the present invention also provides applications of organic conductive gel in flexible electrodes, sensors, wearable devices, and soft robots. Beneficial Effects
[0010] (1) The preparation method of the organic conductive gel of the present invention is simple and safe, the acrylamide self-polymerization reaction system is simple, the reaction process is mild and controllable, and it can be made into various forms according to application requirements, which is conducive to mass production; (2) The organic conductive gel of the present invention is soft and transparent, has good tensile elasticity, good frost resistance, good self-healing property, good conductivity and stability, and strong adaptability, and can be widely used in the fields of flexible electronic devices, electrodes, sensors, wearable devices and soft robots. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 is the tensile property of the organic conductive gel of Example 1; Figure 2 The conductive path of the organic conductive gel of Example 1 was illuminated by an LED lamp. Implementation
[0012] The present invention is further described below in conjunction with specific embodiments, which are not intended to limit the present application. Example 1
[0013] Dissolve 1g of oxalic acid in 1g of propylene glycol, add 0.22g of potassium bromide, stir and dissolve, and obtain a mixed organic solution A. Dissolve 1.11g of acrylamide powder in 1.11g of propylene glycol to obtain an organic solution B. Mix organic solution B and organic solution A and stir until uniform, vacuum degas, and stand at room temperature for 60 minutes, so that acrylamide polymerizes to obtain a soft and transparent organic conductive gel. Figure 1 It can be seen that the organic conductive gel has good stretchability. Figure 2 It can be seen that the circuit formed by the organic conductive gel successfully lights up the LED bulb, indicating that it has good conductivity. Example 2
[0014] 1g of oxalic acid was dissolved in 3g of propylene glycol, and 1g of lithium bromide was added thereto, and the mixture was stirred and dissolved to obtain a mixed organic solution A. 3g of acrylamide powder was dissolved in 2g of propylene glycol to obtain an organic solution B. The organic solution B was mixed and stirred with the organic solution A until uniform, vacuum degassed, and allowed to stand at room temperature for 60 minutes, so that the acrylamide was polymerized to obtain a transparent organic conductive gel. Example 3
[0015] 1 g of tartaric acid was dissolved in a mixture of 1.5 g of propylene glycol and 1.5 g of ethylene glycol, and 0.4 g of lithium bromide and 0.1 g of sodium dihydrogen phosphate were added thereto, and the mixture was stirred and dissolved to obtain a mixed organic solution A. 5.4 g of acrylamide powder was dissolved in 3.6 g of ethylene glycol to obtain an organic solution B. Organic solution B was mixed and stirred with organic solution A until uniform, vacuum degassed, and allowed to stand at room temperature for 120 min to polymerize acrylamide to obtain a transparent organic conductive gel. Example 4
[0016] 1 g of malic acid was dissolved in 2 g of ethylene glycol, and 0.53 g of lithium bromide was added thereto, and the mixture was stirred and dissolved to obtain a mixed organic solution A. 3 g of acrylamide powder was dissolved in 2.3 g of ethylene glycol to obtain an organic solution B. The organic solution B was mixed and stirred with the organic solution A until uniform, vacuum degassed, and allowed to stand at room temperature for 180 min, so that acrylamide was polymerized to obtain a transparent organic conductive gel. Example 5
[0017] 1 g of oxalic acid was dissolved in 2 g of propylene glycol, and 0.6 g of lithium bromide and 0.15 g of sodium chloride were added thereto, and the mixture was stirred and dissolved to obtain a mixed organic solution A. 4.5 g of acrylamide powder was dissolved in 3 g of propylene glycol to obtain an organic solution B. The organic solution B was mixed and stirred with the organic solution A until uniform, vacuum degassed, and allowed to stand at room temperature for 60 min, so that the acrylamide was polymerized to obtain a transparent organic conductive gel.
Claims
1. A method for preparing an organic conductive gel, characterized in that: The steps include: S1. dissolving a metal salt and a low polycarboxylic acid in a low polyol to obtain a mixed organic solution A, wherein the metal salt is one or more of lithium bromide, lithium chloride, potassium bromide, potassium chloride, sodium chloride, and sodium dihydrogen phosphate; the low polycarboxylic acid is any one of oxalic acid, malic acid, and tartaric acid; and the low polyol is one or more of ethylene glycol, propylene glycol, and glycerol; S2. dissolving acrylamide powder in a lower polyol to obtain an organic solution B, wherein the lower polyol is one or more of ethylene glycol, propylene glycol and glycerol; S3. Mix the organic solution A and the organic solution B, stir them evenly, degas them in vacuum, and let them stand for a short time to allow the acrylamide to polymerize and generate polyacrylamide organic conductive gel.
2. The method for preparing the organic conductive gel according to claim 1, characterized in that: The amount of the metal salt in S1 is 10 wt%~20 wt%.
3. The method for preparing the organic conductive gel according to claim 1, characterized in that: The mass ratio of the lower polycarboxylic acid to the lower polyol in S1 is 1:1-3.
4. The method for preparing the organic conductive gel according to claim 1, characterized in that: The mass ratio of acrylamide to low polyol in S2 is 1-1.5:
1.
5. The method for preparing the organic conductive gel according to claim 1, characterized in that: The mass ratio of the organic solution A to the organic solution B in S3 is 1:1-2.
6. Application of the organic conductive gel obtained by the preparation method of the organic conductive gel according to claim 1 in flexible electrodes, sensors, wearable devices, and soft robots.